Disaster! Ive just dropped a piece of greenware and it broke in two places. Clean break but it was made by somebody else as apresent for her Dad!!
Is there any way of repairing it or will I have to own up? ThanksPosted Image

#2 bciskepottery

bciskepottery

    Advanced Member

  • Moderators
  • 1,974 posts
  • LocationNorthern Virginia

Posted 27 August 2012 - 06:14 AM

I was in a handbuilding class with Alfredo Ratinoff and watched him repair a student's greenware earthenware bowl that was broken in several pieces . . . he misted/wrapped the edges with damp towel until they were soft enough to work with, then scored and slipped, then reassembled . . . one piece at a time. Over the course of about three hours, he rebuilt the bowl. Was fascinating to watch (I got no almost no work done that night but learned a lot watching). Not sure if it can be done in your case, though. When Alfredo was studying in Italy, he did statue restoration . . . so he really knew how to do such a repair.

#3 Marcia Selsor

Marcia Selsor

    Professor Emerita, Montana State University-Billings

  • Members
  • PipPipPip
  • 4,645 posts
  • Locationwhere Texas, Matamoros, Rio Grande and Gulf of Mexico come together.

Posted 27 August 2012 - 07:32 AM

Use a toilet paper /paper clay patch. Mix it up in the blender.
Mix
your clay in dry powder form, dash of vinegar, drop or two of sodium silicate
toilet paper that has soaked overnight
stir in the blender. Use about 15% tp to your volume of powdered clay.
dampen the edges before applying.
Marcia

#4 ~janie

~janie

    ~janie

  • Members
  • PipPipPip
  • 103 posts
  • LocationHot old Texas Coast

Posted 27 August 2012 - 11:39 AM

What Marcia said. Do be sure your edges are nicely damp. I use paper clay for all repairs in my studio.

#5 morah

morah

    Educator who is just learning about ceramics

  • Members
  • PipPipPip
  • 51 posts

Posted 27 August 2012 - 07:54 PM

Use a toilet paper /paper clay patch. Mix it up in the blender.
Mix
your clay in dry powder form, dash of vinegar, drop or two of sodium silicate
toilet paper that has soaked overnight
stir in the blender. Use about 15% tp to your volume of powdered clay.
dampen the edges before applying.
Marcia


Marcia, I am sorry to be such a novice but would you mind explaining about powdered clay? Do you just save the dried up clay powder (that I thought I should avoid because its not safe to breathe) or is there some process to make it? Also, is there any particular type of vinegar- wine, white, etc.? And last but not least, what is sodium silicate and where do you get it? Thanks. Morah

#6 Marcia Selsor

Marcia Selsor

    Professor Emerita, Montana State University-Billings

  • Members
  • PipPipPip
  • 4,645 posts
  • Locationwhere Texas, Matamoros, Rio Grande and Gulf of Mexico come together.

Posted 27 August 2012 - 09:16 PM

Morah,
The easiest way to mix your patch without excessive water is to take dried crumbs of theclay being repaired, crush it with a rolling pin,a mallet, the back of a spoon so that your end result is powder. Hope this explains it. you don't want to usewateryslip because there's too much water with theclay.

Marcia

#7 Mark C.

Mark C.

    Advanced Member

  • Members
  • PipPipPip
  • 3,906 posts
  • LocationNear Arcata Ca-redwood rain forest

Posted 27 August 2012 - 09:24 PM

One other choice you have that has worked well for us in small repairs is an Amaco product called SP -mender for greenware as well as better luck with
Aztec-high fire mender as you mix it with your dry clay body.It works up thru all cone temps.
Mark
Mark Cortright
www.liscomhillpottery.com

#8 TJR

TJR

    Advanced Member

  • Members
  • PipPipPip
  • 1,651 posts
  • LocationCanada

Posted 27 August 2012 - 09:39 PM

This is what you want for greenware repairs.It is called spooze.
1 Several tablespoons of your clay body, CRUSHED AS A DRY POWDER.
2. two tablespoons of white vinegar.
3.Caro syrup-a tablespoon or some other cheap syrup.
Mix it up like a paste. Repair the work. Do not store it as it stinks from the syrup rotting.
Good luck.
TJR.

#9 morah

morah

    Educator who is just learning about ceramics

  • Members
  • PipPipPip
  • 51 posts

Posted 27 August 2012 - 10:01 PM

This is what you want for greenware repairs.It is called spooze.
1 Several tablespoons of your clay body, CRUSHED AS A DRY POWDER.
2. two tablespoons of white vinegar.
3.Caro syrup-a tablespoon or some other cheap syrup.
Mix it up like a paste. Repair the work. Do not store it as it stinks from the syrup rotting.
Good luck.
TJR.


Thanks TJR. Caro syrup sounds a lot more familiar then sodium silicate! Do you also put toilet paper into this mixture?

#10 Marcia Selsor

Marcia Selsor

    Professor Emerita, Montana State University-Billings

  • Members
  • PipPipPip
  • 4,645 posts
  • Locationwhere Texas, Matamoros, Rio Grande and Gulf of Mexico come together.

Posted 28 August 2012 - 06:26 AM

Spooze is the best recipe IMHO. Just go easy on the corn syrup.
I like vinegar instead of water. and yes on the toilet paper.


Marcia

#11 eoteceramics

eoteceramics

    Advanced Member

  • Members
  • PipPipPip
  • 66 posts

Posted 29 August 2012 - 02:26 AM

Wow thanks for all the replies!

This forum is a lifesaver, Im going to try the suggestions on a few scraps of greenware before
attempting the actual piece. i think I will have to tell her that it broke whatever the outcome.
Hopefully it will be a good one! Thanks again, will post how I got on.



#12 Earth and Fire

Earth and Fire

    Newbie

  • Members
  • Pip
  • 2 posts

Posted 12 November 2012 - 05:59 AM

This is what you want for greenware repairs.It is called spooze.
1 Several tablespoons of your clay body, CRUSHED AS A DRY POWDER.
2. two tablespoons of white vinegar.
3.Caro syrup-a tablespoon or some other cheap syrup.
Mix it up like a paste. Repair the work. Do not store it as it stinks from the syrup rotting.
Good luck.
TJR.


Hi !

I have problems with very small cracks appearing on a piece which isn't completely dry yet. They appear there where two parts join and I am suspecting one wasn't as soft as the other while joining them ... classic beginners problem :-S ... I fear that it will completely crack while bone-dry.
I tried scoring, humidifying, consolidating the area with soft clay, but after leaving it to dry slowly (wrapped in plastic), they still come through (smaller, but still).
Your solution seems worth trying. Is this a good way to proceed : scoring, humidifying, putting on some of the paste and than later on sanding off the excess ?

Thanks for your help !

Chris

#13 Benzine

Benzine

    Socratic Potter

  • Members
  • PipPipPip
  • 2,086 posts
  • LocationThe Hawkeye State

Posted 12 November 2012 - 06:27 PM

I'm a fan of "Ceramic Enhancer", which can be used to mend dry pieces of clay, though I may have to try some of those other recipes.
My Ceramics instructor in college, told me about using Karo syrup mixed with clay powder, but it didn't have the vinegar in it.
"Anything worth believing, is worth questioning"

#14 Earth and Fire

Earth and Fire

    Newbie

  • Members
  • Pip
  • 2 posts

Posted 13 November 2012 - 04:39 AM

I'm in France and I am not sure to find Ceramic Enhancer here ... same for the Karo Syrup. I tried another kind of candi syrup.

#15 Karen B

Karen B

    Potter 1981-present

  • Members
  • PipPipPip
  • 215 posts
  • LocationMassachusetts

Posted 13 November 2012 - 08:45 AM

I'm in France and I am not sure to find Ceramic Enhancer here ... same for the Karo Syrup. I tried another kind of candi syrup.


Karo Syrup is actually corn syrup.

#16 yedrow

yedrow

    Advanced Member

  • Members
  • PipPipPip
  • 405 posts

Posted 13 November 2012 - 01:01 PM

Thanks Marcia and TJR. I think I've written these solutions in some form down three times already, perhaps at some point I'll be able to find one quickly.

Joel.

#17 SmartsyArtsy

SmartsyArtsy

    Chris Seminara

  • Members
  • PipPipPip
  • 182 posts
  • LocationPNW

Posted 13 November 2012 - 11:34 PM

Just a caution about buying Sodium Silicate. In my local drugstore, It is 5x the price I buy it for at a ceramic supplier-- 400% MORE! So, it is worth checking carefully




0 user(s) are reading this topic

0 members, 0 guests, 0 anonymous users