Min Posted April 5, 2015 Report Share Posted April 5, 2015 I have 2 glazes with the same colourants, 1 results in a amber colour with no iron speckles, the other is full of speckles. Same claybody, firing schedule used for both glazes. I know I could probably ball mill the speckled one but I'm wondering what is causing the iron to agglomerate in the glaze? ^6 electric, low coe glazes. no iron speckles recipe: Tea Silica 23.00 EP Kaolin 14.00Nepheline Syenite 10.00Frit 3195 16.603134 4.80Australian Spodumene 15.00Dolomite 15.00 Bentonite 2.00Manganese Dioxide 3.00Iron Oxide Red 2.00105.40 Speckles Silica 34.50Wollastonite 5.00EP Kaolin 23.00Minspar 12.00Gerstley Borate 22.00Talc 3.00Dolomite 3.00Nepheline Syenite 2.90 Manganese Dioxide 3.00 Iron Oxide Red 2.00 I don't think the higher silica levels in the second recipe is the culprit, I'm thinking the lithia in the first recipe might have something to do with it? Boron differences? Any thoughts most welcome. Link to comment Share on other sites More sharing options...
High Bridge Pottery Posted April 5, 2015 Report Share Posted April 5, 2015 Interesting, got any pictures? I have no real ideas My though process would be the first glaze melt is managing to incorporate all the iron and manganese into the melt and the second glaze is not. Can't back this up with much information, just a guess. It could be manganese speckles and not iron. Link to comment Share on other sites More sharing options...
Min Posted April 5, 2015 Author Report Share Posted April 5, 2015 If it helps, first pic is the "Tea" glaze, second is the one I'm trying to rid of specks. Also, same batch of RIO and Manganese. I'm stumped. Madeleine Link to comment Share on other sites More sharing options...
bciskepottery Posted April 5, 2015 Report Share Posted April 5, 2015 Wondering if the amber glaze (no specks) is a better melter than the one with specks? The amber has a lot of fluxes (spodumene, neph sye, frits) that might be better at melting the oxides than the second glaze. Link to comment Share on other sites More sharing options...
High Bridge Pottery Posted April 5, 2015 Report Share Posted April 5, 2015 I love the speckle It could be to do with the high silica/borate. Doing some crude calculations you seem to be at the upper limits of cone 6 glazes for both. "Crystals are normally silicate or borate compounds, thus SiO2 and B2O3 need to be present in significant amounts." http://digitalfire.com/4sight/glossary/glossary_devitrification_crystallization.html Now is the speckle a crystal, I do not know. To me it would come from adding some granular manganese but seeing as you are using the same for both glazes I am stumped. Link to comment Share on other sites More sharing options...
Judith B Posted April 6, 2015 Report Share Posted April 6, 2015 I like the speckles a lot too! Link to comment Share on other sites More sharing options...
Tyler Miller Posted April 6, 2015 Report Share Posted April 6, 2015 My money's on the frits being the difference. Link to comment Share on other sites More sharing options...
Diz Posted April 6, 2015 Report Share Posted April 6, 2015 Min - both are good looking glazes! Thanks for sharing - the speckled one catches my eye! Link to comment Share on other sites More sharing options...
Min Posted April 6, 2015 Author Report Share Posted April 6, 2015 Thanks for your thoughts. Back to the drawing board, well back to the glaze testing I guess. Link to comment Share on other sites More sharing options...
jrgpots Posted April 8, 2015 Report Share Posted April 8, 2015 Wallastonite can have many impurities,such as garnet as mentioned in digitalfire. Could this be the source of your specks? I would try a different source of this ingredient. That's my guess. Jed Link to comment Share on other sites More sharing options...
David Woodin Posted April 8, 2015 Report Share Posted April 8, 2015 It is the talc in the glaze. David Link to comment Share on other sites More sharing options...
Min Posted April 8, 2015 Author Report Share Posted April 8, 2015 Wallastonite can have many impurities,such as garnet as mentioned in digitalfire. Could this be the source of your specks? I would try a different source of this ingredient. That's my guess. Jed Thanks for the idea but I don't think it's the wollastonite as I use some from the same batch in another glaze with no specks. I just got the last bag of the old supply from my supplier, don't know how different the new stuff will be. Link to comment Share on other sites More sharing options...
Min Posted April 8, 2015 Author Report Share Posted April 8, 2015 It is the talc in the glaze. David Even though the MgO supplied to both recipes is exactly the same? I will omit the talc and replace with more dolomite and adjust the silica and calcium levels and see. Thanks for the thought. It seems the consensus is it could be anything and everything except the silica, spar or kaolin. Lots of fun. I think I might just scrap the speckled glaze and start over but I would like to know the cause of the specks for glaze testing going forward. Or to look at the other way around, why there are no specks in the first glaze. Link to comment Share on other sites More sharing options...
David Woodin Posted April 8, 2015 Report Share Posted April 8, 2015 Sorry, before looking at the pictures I though you were talking about teadust. MGO will produce teadust in some glazes. The speckles glaze is on the AL/SI outer limits and B203 is quite high. Both glazes use a lot of different materials. They both could be modified so that you would not have to stock so many materials. Neither is in the food safe limits. I am not much help. David Link to comment Share on other sites More sharing options...
Min Posted April 8, 2015 Author Report Share Posted April 8, 2015 Hi David, Which limit figures are you using that have them both coming up outside the limits? Using Insight and the Hesselberth/Roy limits plus the Green/Cooper ones the silica and boron are high in the speckled one, I have the first one coming within the limits. That second one, the Speckles, is my version of G1215U Low Expansion from Tony Hansen at Digitalfire where I removed the 3249 frit and rebalanced the formula. I used the original G1215U for a few years but that frit is so expensive I have redone the recipe without it. Without the colourants the 2 versions are very close. I have never considered high silica levels to be a problem if there is a good melt, as Hansen is okay with these silica and boron levels I wasn't concerned with them being what they are.This is what I get for the unity formulas: Tea: CaO 0.40*Li2O 0.11*MgO 0.25*K2O 0.02*Na2O 0.12*P2O5 0.00*TiO2 0.00Al2O3 0.40B2O3 0.21SiO2 2.80Fe2O3 0.04MnO 0.00*MnO2 0.10* and the Speckled one: CaO 0.51*MgO 0.22*K2O 0.03*Na2O 0.12*P2O5 0.00*TiO2 0.00Al2O3 0.42B2O3 0.31SiO2 3.81Fe2O3 0.05MnO2 0.13* Yup, if I used a lot of the first glaze I would rework the recipe but haven't bothered. I use all those materials in other glazes so it's no bigs. Thanks for your thoughts, Madeleine Link to comment Share on other sites More sharing options...
Babs Posted April 8, 2015 Report Share Posted April 8, 2015 does the speckle occur without the colourants ie in the base glaze? or without the iron etc.... Link to comment Share on other sites More sharing options...
Min Posted April 9, 2015 Author Report Share Posted April 9, 2015 does the speckle occur without the colourants ie in the base glaze? or without the iron etc.... base glaze is crystal clear, it's a terrific low coe base which I modified from this one: http://digitalfire.com/4sight/recipes/low_expansion_glossy_clear_cone_6_45.html (it will likely shiver or dunt on a lot of stonewares so if anyone tries it please test for this) Link to comment Share on other sites More sharing options...
High Bridge Pottery Posted April 9, 2015 Report Share Posted April 9, 2015 Have you tried both glazes with different colourants to see what happens? I think it could be the high b2o3 with the silica and high cao crystallizing something out the melt. Could try reducing the b2o3 and adding some other flux. Lots of speculation in here but great ideas to test out. Why do you want this other glaze to 'work'? Interesting to see the pic on digital fire with mason stains, do the browns there have a slight speckle? I can see something. Maybe removing the frit has enhanced it along with using raw oxides. Have you tried the recipe with the frit before you rebalanced it? Link to comment Share on other sites More sharing options...
Min Posted April 9, 2015 Author Report Share Posted April 9, 2015 Hi High Bridge, I'm mostly trying to figure out the "why" of this. I've had other glaze tests speckle and have often wondered why some do and some don't. I'll add a test tile with original G1215U plus colourants in the next glaze fire, I hadn't done that since I'm trying to get away from using the expensive frit that it uses but it might answer the question. Glaze testing sure takes up a lot of time doesn't it? Link to comment Share on other sites More sharing options...
David Woodin Posted April 9, 2015 Report Share Posted April 9, 2015 Probably some of my materials are not up to date.. Tea using Matrix, all within limits, Green and Cooper in limits, Food safe Alumina okay, Silica too high, Insight Alumina too high SI okay MGO high KNO low B203 low. Speckles, Matrix AL okay Si on the edge of being too high, Food Safe AL too high Si on the edge, Green and Cooper B203 on the edge of being high, Insight AL and Si high B203 low MGO high KNO low. So it is best to use what you are satisfied with. David Link to comment Share on other sites More sharing options...
Min Posted April 10, 2015 Author Report Share Posted April 10, 2015 Thanks for taking the time to enter all that David. I need low coe glazes so MgO being high at the expense of the lower K2O is what that formula was trying to achieve. If I ever work my way through this I'll post results. Link to comment Share on other sites More sharing options...
Guest JBaymore Posted April 10, 2015 Report Share Posted April 10, 2015 Has the speckled glaze batch been stored wet for any amount of time or is it speckling when first mixed? best, ....................john Link to comment Share on other sites More sharing options...
Min Posted April 10, 2015 Author Report Share Posted April 10, 2015 It was mixed and applied to test tiles straight away. I mix the glaze up then put through a 80 mesh sieve. Speckles were not apparent in glaze slurry that is why I am wondering if the iron is agglomerating during the firing? I've always thought RIO is very fine particled, the speckles are fairly large. I think the only way I'm going to solve this is change one material at a time as see what happens. Crazy at home right now so this might get pushed onto the back burner as it's more about the theory than practice. Link to comment Share on other sites More sharing options...
rayaldridge Posted April 13, 2015 Report Share Posted April 13, 2015 You must be a more confident glaze mixer than me. My first thought would be that I had made a mistake in the materials I added to the glaze. Have you tried mixing up a hundred grams of the glaze and testing it, just to be sure Link to comment Share on other sites More sharing options...
jrgpots Posted April 13, 2015 Report Share Posted April 13, 2015 I remember an organic chem lab I had to take. I made vanilla crystals which normally are large and white. Mine were small and green. The size came from being too much in a hurry. I can buy that....But the green color? The mass spectrometer showed copper in the mix. It turned out that I used an old chrome plated scoop to measure ans stir my soln. The chrome had worn off and the copper metal was exposed to the acidic solution. The result...green crystals. It comes to mind every time I have an unusual outcome. When it comes to glaze making, it is ever present on my mind. Just reflections. Jed Link to comment Share on other sites More sharing options...