mikenightmare Posted December 4, 2013 Report Share Posted December 4, 2013 I am a high school ceramics teacher (this is my first year doing ceramics in 6 years after a transfer within my district) so I am relearning everything about ceramcis, and kiln firing is very new for me. The school has a Geil gas kiln. I am (attempting) cone 10 reduction firing and I can not get Vegas Red to come out red. One piece came out transparent (middlish-front of the kiln). There were a couple that were towards the bottom back of the kiln that had some red come out. I am following a schedule I found in a notebook from the previous teacher. It fires around 12 hours. The glaze is the premixed glaze from aardvark. I hope this is enough information to help me out I am not sure if I am getting into reduction properly or not. Any help would be great, if I need to provide more information please let me know. Like I said this is new for me and trying to figure it all out. Thanks, Michael Link to comment Share on other sites More sharing options...
bciskepottery Posted December 5, 2013 Report Share Posted December 5, 2013 Assuming Vegas Red is a copper red, that white to transparent result generally is a sign of more oxidation during firing and not enough reduction. Copper reds like reduction; copper reds also fume during firing. I've had my best results using copper reds on interiors where the fumes tend to keep inside the pot. Link to comment Share on other sites More sharing options...
mikenightmare Posted December 5, 2013 Author Report Share Posted December 5, 2013 Thank you for the reply @bciskepottry Assuming Vegas Red is a copper red, that white to transparent result generally is a sign of more oxidation during firing and not enough reduction. Copper reds like reduction; copper reds also fume during firing. I've had my best results using copper reds on interiors where the fumes tend to keep inside the pot. Link to comment Share on other sites More sharing options...
oldlady Posted December 5, 2013 Report Share Posted December 5, 2013 Geil is very helpful to users. contact them or perhaps Tom Coleman, another in the long list of very helpful people. the Vegas Red is his formula. see the 2010 cad discussion re Vegas red and read the comments below the article. tom answered someone about the firing schedule. where are you? is there a studio potter nearby whose firing you could watch and learn from? you do know that you are attempting the most difficult color to achieve. Link to comment Share on other sites More sharing options...
mikenightmare Posted December 5, 2013 Author Report Share Posted December 5, 2013 Thanks for the tip on the article I found it and his response is helpful on there. I am in so cal. Close to Geil actually. I think I will give it another go with my new info and see what happens then try contacting Geil for some advice. And yes I do know reds are hard to achieve bit I like to challenge myself and figure things out and master difficult task. Hopefully this will be one of them. Link to comment Share on other sites More sharing options...
Marcia Selsor Posted December 5, 2013 Report Share Posted December 5, 2013 I fired vegas Red in a big old Olsen updraft two years ago when I was teaching at UTB. The kiln was 20+ years old, rusted air discs on the end of all 14 venturi burners. I followed the previous instructors kiln logs and the kiln fired like a dream.We got reds. As Bciske says, the outer areas of the stacking may not reduce as well.Pack it tight. Also, when doing reds, it is good to start a gentle reduction about ^09 and stay neutral going up. reduce more heavily around 8,9,10. Not necessary for black smoke but it depends on your gas. Natural gases vary quite a lot.You can test for oxygen by holding a stick in front of the peep holes. If they don't burn, you are reducing.Sometimes there is a purple green flame. Just for the sake of the kiln Gods , I would feed small sticks through the peepholes as it started to cool. Maybe a few every 1/2 hour for the first 2 hours of cooling. Just kiln lore but I believe. Marcia Link to comment Share on other sites More sharing options...
neilestrick Posted December 6, 2013 Report Share Posted December 6, 2013 Copper reds often need to be applied thickly, which can make them run more, so watch out. Keep them away form the burner areas. If they go too hot they will burn out to clear. There is very little copper in the glaze, and it fumes out during the firing. I think you probably reduced fine, because when they oxidize they go green, not clear. Apply thicker, try firing 1/2 cone cooler, and fire faster if possible. Link to comment Share on other sites More sharing options...
Guest JBaymore Posted December 6, 2013 Report Share Posted December 6, 2013 Neil likely has it. best, ................john Link to comment Share on other sites More sharing options...
mregecko Posted December 6, 2013 Report Share Posted December 6, 2013 It's been a while since I've done ^10 reduction, but I definitely agree with the thicker application on copper reds. It makes a huge difference. And yes, they can run too. I've also had really good luck with putting a celadon glaze (or a clear) over copper reds. I'm not sure of the mechanic, maybe it reduces the availability of oxygen to the copper in the copper red, or maybe it's just superstition... But it seemed to work for me before. Link to comment Share on other sites More sharing options...
Marcia Selsor Posted December 6, 2013 Report Share Posted December 6, 2013 I agree with the thickness of copper red. Here are some Vegas Red pieces from the old Olsen I fired at UTB.There are 4 columns of shelves. This is student work. In the closeup, the pot on the left is stoneware. The pot on the right is porcelain. In the center bottom there are some textured pots which respond well breaking clear on the surface of porcelain. Vegas red is a beautiful glaze when it works.This firing was about 11 hours.You can see two cone packs if you look close. ^10 is standing, ^9 is down. even top and bottom. Marcia Link to comment Share on other sites More sharing options...
mikenightmare Posted December 8, 2013 Author Report Share Posted December 8, 2013 thanks for thr replies . Neil your response is helpful. there were aa couple pieces in the bottom that had some of the red come out which is generally cooler than the bottom so it sounds like i am not far off from getting them to come out . thanks everyone! Link to comment Share on other sites More sharing options...