Bam2015 Posted April 13 Report Share Posted April 13 My satin glaze is not playing nice with Amaco black or Coyote black underglazes, or maybe it's the other way around. Does anyone know what the problem could be? The recipe from Glazy.org Ferro Frit 3124 36 Wollastonite 27 EPK 35 Silica 5 The person who contributed this recipe states that it adds up to 103. Betty Quote Link to comment Share on other sites More sharing options...
Jarman Porcelain Posted April 13 Report Share Posted April 13 Do you have photos or a detailed description of what is happening? There isn't enough information here to help you. Quote Link to comment Share on other sites More sharing options...
Bam2015 Posted April 13 Author Report Share Posted April 13 I don't have a picture, but they are pinholes. Sorry, should have mentioned that. It's actually a sort of cool look. Are pots with pinholes food safe? Thanks, Betty Quote Link to comment Share on other sites More sharing options...
Min Posted April 13 Report Share Posted April 13 Are you bisque firing the underglaze on before glazing? Quote Link to comment Share on other sites More sharing options...
Bam2015 Posted April 13 Author Report Share Posted April 13 Min, I am applying the underglaze in the greenware stage then bisque firing to 04, glaze fire to 6. I have an L & L kiln and use their programs for slow bisque and slow glaze. Betty Roberta12 1 Quote Link to comment Share on other sites More sharing options...
Roberta12 Posted April 14 Report Share Posted April 14 @Bam2015One technique that has helped me is to lightly rub a finger over the underglazed areas, after you have brushed/dipped/sprayed your satin or glossy glaze. I think it is to smooth it out and make sure the glaze covers the ug. Rae Reich 1 Quote Link to comment Share on other sites More sharing options...
Rae Reich Posted April 14 Report Share Posted April 14 You might try slightly dampening the black areas of the bisque before applying the glaze. Blot with a sponge for small areas or a quick dip in water. Quote Link to comment Share on other sites More sharing options...
Jarman Porcelain Posted April 14 Report Share Posted April 14 https://insight-live.com/insight/share.php?z=7WnpT9vC3b This has some great info on your glaze, as well as multiple revisions meant to solve known issues. Hulk, PeterH and Rae Reich 3 Quote Link to comment Share on other sites More sharing options...