Testing a new glaze firing schedule. Trying to rid myself of microdimples when working with good ole GB.
- Show previous comments 2 more
-
i found a firing schedule from Perry at Skutt for ^5, just take it to your cone temp.. ill try to post it in my gallery..
-
segment 1 rate 200 Temp 250 hold none
Segment 2 Rate 400 Temp 1000 no hold
Segment
Segment 3 Rate 180 Temp 1150 no hold = adjust if you are need/want more burn off..
Segment 4 Rate 300 Temp 1967 Hold none
Segment 5 120 Temp 2160 {^5} adjustable =Hold 5 minutes
Segment 6 Rate 125 Temp 1900 Hold 45 minutes
-