I am squeezing out a glaze formulated for majolica.

 

San Diego State U Majolica - C 6

Dolomite 2.3

Whiting 8.7

 Feldspar 35.8

EPK 5.8

Flint 35.7

frit 3124 10.5

Zircopax 1

Bentonite 2

Epsom salts 0.6 

Edited by docweathers
add info

Share this post


Link to post
Share on other sites

My thought would be it's going on too thick. I would try watering it down then, (if necessary) adding just enough more epsom salts solution to thicken it up enough to trail without it running off the pot. 

3 hours ago, docweathers said:

I am usually working on ^6 bisque

Did you mean ^6 clay bisqued to ^04 or thereabouts? You are trailing on bisque, not a base glaze?

Share this post


Link to post
Share on other sites

Is the effect you get similar to tube-lining (like Moorcraft style)? A recipe for the thick 'outlining' glaze, from a book of mine, haven't yet tried it--

36 kaolin

36 quartz

16 ball clay

4 whiting

4 standard boron frit

4 high alkaline frit

Share this post


Link to post
Share on other sites
8 hours ago, NancyAmores said:

Is the effect you get similar to tube-lining (like Moorcraft style)? A recipe for the thick 'outlining' glaze, from a book of mine, haven't yet tried it--

36 kaolin

36 quartz

16 ball clay

4 whiting

4 standard boron frit

4 high alkaline frit

Thanks for sharing the recipe but looks like a  slip / engobe rather than a glaze.

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now

×

Important Information

By using this site, you agree to our Terms of Use.