KB3d Posted April 4, 2023 Report Share Posted April 4, 2023 I would like to mix the slip recipe by Susan Feagin in Ceramic Recipies. Susan writes:”For batching: I weigh out the ingredients and make a 5000-gram dry-mix batch. When I’m ready to make colors, I measure out a 500-gram portion of the dry mix into a container, measure out dry Mason stains, and add that to the dry-mix slip base. Then I add water, mix, and sieve to make the slip smooth and perfect for brushing.” I am wondering, how would I mix the 5000-grams of dry ingredients thoroughly enough to use small portions, without creating airborne chemicals? Thanks, Karen Borg Quote Link to comment Share on other sites More sharing options...
Callie Beller Diesel Posted April 4, 2023 Report Share Posted April 4, 2023 If you’re wanting to mix a large master batch that then gets divided out, leave out the dry mixing entirely, but weigh the water. If you know how much water went into the batch you can divide it out evenly. If you keep to metric measurements, this will be easier, because 1 ml of water weighs 1 gram. It doesn’t work like that for all fluids, but it does for water. If you are used to using a measuring cup, check how accurate it is by filling it to a given measurement line and weighing it to make sure it’s close enough for your purposes. For instance, if you add 2500 g of water to your 5000g batch, the whole thing will weight 7500g, so a quantity of slip that weighs 1500g will contain 1000g of slip base. (Numbers made up off the top of my head for ease. You may have to play with your water additions to get your consistency right. Just record what you did.) From there, you can add your colourants to portions of your master batch. To mix thoroughly, you will need to use a stick blender that rotates really fast. If you use something slower like a jiffy mixer, you’ll have to let it mix a lot longer to get everything distributed properly. For some colourants that don’t break up easily, you may have to sieve the mix again. Roberta12, Rae Reich, High Bridge Pottery and 1 other 4 Quote Link to comment Share on other sites More sharing options...
Min Posted April 4, 2023 Report Share Posted April 4, 2023 Another option would be to put the full 5kg batch into a pail with a lid that can be sealed on (twist type pail lid) then roll it and flip it around for 15 minutes or so. Leave the pail sit for a day for all the dust inside to settle then scoop it out just like any other dry material. If it sits for a while then roll it around again before using. I do smaller 500 gram test batches of base glazes like this all the time using a large freezer ziplock bag. Hulk, Roberta12 and Rae Reich 3 Quote Link to comment Share on other sites More sharing options...
High Bridge Pottery Posted April 4, 2023 Report Share Posted April 4, 2023 (edited) @Callie Beller Diesel You could write it out as: dry weight = portion weight / total weight x batch weight You could either work it out per bucket of slip or make sure to take the dry weight off the batch weight for next time you work it out. Using Callie's example ~ 1500 / 7500 x 5000 = 1000 if you wanted to keep working it out every time you need to take off the 1000 of dry weight from the batch weight for next time so it would be 1500 / 6000 x 4000 = 1000 (assuming you haven't lost water to evaporation) If the slip is thin enough to measure the volume accurately you can weigh a volume of slip and then (volume of slip weight - same volume of water weight) x 5/3 = dry weight If you can measure the specific gravity and know what dry weight you need you can also work out what volume of slip you want with volume needed = (3 x dry weight) / ((5 x specific gravity) -5) Edited April 4, 2023 by High Bridge Pottery Hulk 1 Quote Link to comment Share on other sites More sharing options...
KB3d Posted April 4, 2023 Author Report Share Posted April 4, 2023 Thanks Min. And thanks Calle and High Bridge Callie Beller Diesel and Hulk 2 Quote Link to comment Share on other sites More sharing options...
Recommended Posts
Join the conversation
You can post now and register later. If you have an account, sign in now to post with your account.