Everyone was so helpful with my last question so maybe I can get some help with this problem. This bowl that cracked was a cone 5 clay bisque fired to cone 04. It was dried for a couple weeks and was bone dry. The bottom is probably 1/4 inch thick with a coil rim around the base and the sides taper up from that thickness at the bottom to very thin at the top. Any idea what I did wrong?

thanks

post-45314-0-90942600-1375545665_thumb.jpg

post-45314-0-90942600-1375545665_thumb.jpg

Share this post


Link to post
Share on other sites

Thanks for your help everyone. About 2 hours after the kiln cut off, I pulled the side inspection plugs in the kiln but didn't open the top till morning about 10 hours after it cut off. Maybe it cracked on the side near the plugs.

Share this post


Link to post
Share on other sites

Thanks for your help everyone. About 2 hours after the kiln cut off, I pulled the side inspection plugs in the kiln but didn't open the top till morning about 10 hours after it cut off. Maybe it cracked on the side near the plugs.

 

Probably not.

Share this post


Link to post
Share on other sites

 

Thanks for your help everyone. About 2 hours after the kiln cut off, I pulled the side inspection plugs in the kiln but didn't open the top till morning about 10 hours after it cut off. Maybe it cracked on the side near the plugs.

 

Probably not.

 

Yeah, I would say the same.

 

When I've had cracks like that, it was because I cooled the entire object too quickly, and was probably even foolish enough to take it out of the kiln, and set it on a much cooler surface......I'm like a little kid on Christmas, when it comes to peeking at my work.

Share this post


Link to post
Share on other sites

In my experience, cracks like that happen from cooling issues too. When I do thin raku platters, built in a similar fashion, they crack radially going outwards after being removed from the kiln.

 

I know some people elevate flat pieces like this in the kiln so that they have even airflow all around, and thus even cooling. 

 

So yeah, I'd guess the problem was in the cooling as well.

Share this post


Link to post
Share on other sites

This piece looks thinner than a potato chip on the edge. That makes it very easy to crack just as a real life potato chip. Add this to a thickrt bottom and handling in and out of kiln-also was it a trimmed chip as this also make it easy to crack it. Next time treat it very carfully as any mistreatment will crack that edge.

Mark

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×

Important Information

By using this site, you agree to our Terms of Use.