Looking for a cone 5/6 matte white glaze recipe

Recommended Posts

Natania    6

Anyone know of a good one? I have tried several tests of recipes I've found online mostly, but they are still a bit too glossy for me. Would love to find a good, reliable soft matte white recipe..

Share this post


Link to post
Share on other sites
oldlady    1,323

from george and nancy wettlaufer's book "getting into pots" page 127 CLEAR MATTE

 

 

C6W.....(w for wollastonite) Cone 6

 

 

Kona soda spar.......................33

 

ball clay (C&C is very white).....25

 

zinc oxide...............................12

 

wollastonite............................30

 

the recipe does not call for bentonite but i bet one of our glaze gurus will know if it would help. i think i used 2% when i made this glaze last year. it really is a clear, smooth, matte glaze.

 

because of the zinc oxide i do not use it over green slips or underglazes. they will turn grey.

Share this post


Link to post
Share on other sites
oldlady    1,323

this one is also a great CLEAR glaze but you may have trouble getting Cornwall stone. it also changes green to grey.

 

SATIN MATTE Cone 6

 

dolomite...............20

 

cornwall stone......60

 

EPK....................20

 

for those of you not in the usa, EPK is Edgar Plastic Kaolin. see posts re this stuff...

Share this post


Link to post
Share on other sites
oldlady    1,323

there is a recipe for varigated slate blue in the book Mastering cone 6 glazes. it is a very nice WHITE matte glaze with the Zircopax and rutile. leaving out the additives may make a good clear.

 

VARIGATED BASE GLAZE Cone 6

 

wollastonite........................29

 

nepheline syenite.................4

 

frit 3195..............................20

 

EPK...................................30

 

silica...................................17

..........................................100

 

add

 

rutile................................5%

 

zircopax...........................8%

Share this post


Link to post
Share on other sites
oldlady    1,323

kathy triplett's book contains this recipe. i have made it and like it a lot.

 

Kathy's Stony Matte Cone 6 clear

 

dolomite............................3

 

wollastonite......................22

 

nepheline syenite..............43

 

Kaolin...............................22

 

I do not own this book and only copied out this much so i do not have any description of what kaolin to use. i used EPK.

 

have fun with these.

 

DARN! i just re read the original question and see that it is not for a clear but a white..........

Share this post


Link to post
Share on other sites
Marcia Selsor    1,301

This is a good functional glaze

 

White Liner ^6

 

Ger. Borate 18

Neph. Syenite 27.3

Kaolin 12

Whiting 8.5

Talc 15.6

Silica 9

Zircopax 9

99.4

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×