Caroline E Posted March 14 Report Share Posted March 14 Hi everyone, I am hoping to get some advice regarding a students tile work. Her large tiles had severe cracking/shrinkage from the glaze ^6 oxid. firing (standard ^6 medium speed firing). Please see photo. The student was using commercial clay without grog and used Mayco glazes. For her next set of tiles, I advised the student to use clay with grog and to compress the front/back of tiles. In the firing, we plan to use sand and/or waste slabs underneath the tiles. Is there anything else we should do? Should I be using a firing schedule that has a cooling ramp? Thank you in advance for any help. Caroline Quote Link to comment Share on other sites More sharing options...
neilestrick Posted March 15 Report Share Posted March 15 A waster slab should do the trick, or put some silica sand on the shelf. Make sure you put kiln wash or alumina wax on the waster slab so the tile doesn't stick to it. If you need a cooling ramp it would be during quartz inversion, so from about 1100 to 900, but it's rare that you would need that. Rae Reich and Callie Beller Diesel 2 Quote Link to comment Share on other sites More sharing options...
Caroline E Posted March 15 Author Report Share Posted March 15 @neilestrick Thanks very much. I will try that. Quote Link to comment Share on other sites More sharing options...
Denice Posted March 15 Report Share Posted March 15 I see that there are some cracks running from one lump to another. I make a lot of tile, a thicker area next to a thinner slab can cause cracks to form. She might try removing the clay from the back of the tile in the thick areas and try to keep the clay a even thickness. Denice Rae Reich, Caroline E and Min 3 Quote Link to comment Share on other sites More sharing options...
Caroline E Posted March 18 Author Report Share Posted March 18 @Denice Good point. Thanks! Quote Link to comment Share on other sites More sharing options...
Ben xyz Posted April 9 Report Share Posted April 9 (edited) On 3/14/2024 at 6:30 PM, neilestrick said: A waster slab should do the trick, or put some silica sand on the shelf. Make sure you put kiln wash or alumina wax on the waster slab so the tile doesn't stick to it. Having the same problem with large 14"x20" slab(s), 3/8" thick. I am using recycled studio clay (medium and hi-fire clays mixed together), rotating and flipping the slab often when using the roller (16lbs at a time before trimming). Compressing after with metal rib for further compression before drying. It only occurs when glaze firing (c5) stage and not on bisqued slab (c04). 1. Also making grooves on the back to counter warping (see photo). Perhaps this is making thinner areas against thicker and causing the cracking in half? 2. How do "waster slabs" work? Slightly larger and thicker than initial slab? Placed under bisqued slab? Or under greenware from the beginning? A new process for me. 3. Since these slabs exist as elements in a sculptural piece, I 'm now tempted to glaze fire at a bisque temperature (c04), using a low-fire clear gloss glaze over the underglazed slab and calling it a day. Not as sturdy (w/o full vitrification), but wasting a lot of time, energy and clay from these large slabs cracking in half at c5. Thoughts? Edited April 9 by Ben xyz Clarification Quote Link to comment Share on other sites More sharing options...
neilestrick Posted April 9 Report Share Posted April 9 1 hour ago, Ben xyz said: 2. How do "waster slabs" work? Slightly larger and thicker than initial slab? Placed under bisqued slab? Or under greenware from the beginning? A new process for me. 3. Since these slabs exist as elements in a sculptural piece, I 'm now tempted to glaze fire at a bisque temperature (c04), using a low-fire clear gloss glaze over the underglazed slab and calling it a day. Not as sturdy (w/o full vitrification), but wasting a lot of time, energy and clay from these large slabs cracking in half at c5. Thoughts? The grooves are probably not the issue, and also probably not doing much to prevent warping. Waster slabs can be very thin, and can even be broken/in pieces, but should fully support the piece on it. It's just something that will shrink with the tile and keep the tile from catching on the kiln shelf. Put some kiln wash or alumina wax on the slab so it doesn't fuse to the clay. Waster slab does not need to be bisque fired. No guarantee it won't crack in the second low-fire firing, but it's worth a shot if you don't need the durability of cone 5. It's also possible that your tile is cracking from cooling too quickly, and therefore unevenly, through quartz inversion. You could try a controlled cooling from 1100F down to 850F. Callie Beller Diesel and Ben xyz 2 Quote Link to comment Share on other sites More sharing options...
Recommended Posts
Join the conversation
You can post now and register later. If you have an account, sign in now to post with your account.