SJohnston79 Posted March 9 Report Share Posted March 9 Hello, I am creating a large scuplture built in 19" by 11" sections. I am using 240G standard clay and firing at cone 6. I am now aware this clay body is not a good choice for this sculpture but have a deadline in 2 weeks and have to push on through. With the intent to find a better clay body for the next one. With all that being said I just unloaded a glaze kiln to find the piece totally cracked in half. It had no cracks when it came out of the bisque kiln. Do you have any suggestions on ways to avoid this when I remake this piece? I have attached images. Thanks, Sarah https://imgur.com/aZ2FpZr https://imgur.com/mrXXWB4 https://imgur.com/5weAd1i Quote Link to comment Share on other sites More sharing options...
Callie Beller Diesel Posted March 9 Report Share Posted March 9 Hi and welcome! I wish it was under better circumstances. The pictures are worth a thousand words, and thank you so much for including those! The fact that the piece is broken so cleanly, and in 2 near-perfect vertical lines all the way through means that this wasn’t specifically your clay, or anything you did during building the piece. It’s a nice dense clay that probably stuck to the kiln shelf due to the mass and size of the piece, and cracked during cooling. For the next pieces, I’d fire them on some sand/alumina so that the piece has the equivalent of little refractory ball bearings to shift around on. You could also use a waster slab that will shrink at the same rate as the piece, but take the brunt of the force and absorb the crack instead. If the clay survived the bisque just fine, another possibility is to not fire the piece to full clay maturity. Porosity in the end piece is less of a concern for you than it would be for someone throwing functional ware. neilestrick, Rae Reich, Babs and 1 other 4 Quote Link to comment Share on other sites More sharing options...
Rae Reich Posted March 10 Report Share Posted March 10 Nice work! I like the color, glaze technique and surfaces. Quote Link to comment Share on other sites More sharing options...
SJohnston79 Posted March 11 Author Report Share Posted March 11 On 3/9/2024 at 12:39 PM, Callie Beller Diesel said: Hi and welcome! I wish it was under better circumstances. The pictures are worth a thousand words, and thank you so much for including those! The fact that the piece is broken so cleanly, and in 2 near-perfect vertical lines all the way through means that this wasn’t specifically your clay, or anything you did during building the piece. It’s a nice dense clay that probably stuck to the kiln shelf due to the mass and size of the piece, and cracked during cooling. For the next pieces, I’d fire them on some sand/alumina so that the piece has the equivalent of little refractory ball bearings to shift around on. You could also use a waster slab that will shrink at the same rate as the piece, but take the brunt of the force and absorb the crack instead. If the clay survived the bisque just fine, another possibility is to not fire the piece to full clay maturity. Porosity in the end piece is less of a concern for you than it would be for someone throwing functional ware. Thanks so much for the feedback very helpful Quote Link to comment Share on other sites More sharing options...
Recommended Posts
Join the conversation
You can post now and register later. If you have an account, sign in now to post with your account.