Sharon Posted May 27, 2010 Report Share Posted May 27, 2010 I just dipped my pieces in my glaze and there were a lot of pin holes, so I rinsed off the glaze. Do I need to re bisque fire my piece before I try to glaze it again? The specific Gravity of the glaze is 1.45. Should it be thinner for dipping? Sharon Link to comment Share on other sites More sharing options...
Guest Sherman Posted May 28, 2010 Report Share Posted May 28, 2010 I just dipped my pieces in my glaze and there were a lot of pin holes, so I rinsed off the glaze. Do I need to re bisque fire my piece before I try to glaze it again? The specific Gravity of the glaze is 1.45. Should it be thinner for dipping? Sharon Sharon, Mixing thinner may help, and wetting the bisque first may help as well (particularly if it has a textured surface). Quickly dipping a dry piece of bisque in clean water before dipping into a glaze can sometimes help to "pull" the water in the glaze into all the small nooks and crannies it would otherwise trap air in and therefore not adhere to the piece, causing a hole in the raw glaze. You might also try mixing a very small amount of your glaze with way too much water and either brushing or pouring it over the piece to fill in those spaces, then dip as normal after that initial coat has dried. Hope this helps, Sherman Link to comment Share on other sites More sharing options...
Sharon Posted May 28, 2010 Author Report Share Posted May 28, 2010 I just dipped my pieces in my glaze and there were a lot of pin holes, so I rinsed off the glaze. Do I need to re bisque fire my piece before I try to glaze it again? The specific Gravity of the glaze is 1.45. Should it be thinner for dipping? Sharon Thanks Sherman, I let you Know how this comes out after I fire these pieces. Sharon Link to comment Share on other sites More sharing options...
Plattypus Posted June 16, 2010 Report Share Posted June 16, 2010 Sharon, Have you tried wetting the bisque as Sherman suggested? I have been struggling with pinholes as well.. please post your results if you did. Link to comment Share on other sites More sharing options...
hansen Posted June 17, 2010 Report Share Posted June 17, 2010 Sharon, Have you tried wetting the bisque as Sherman suggested? I have been struggling with pinholes as well.. please post your results if you did. pinholes can come from a variety of sources - Sherman's suggestion is the first line of defense. Also make sure the wares aren't dust covered. And, some clay body formulations promote pinholes, as do certain glaze formulations. Some people like pinholing and might use a punky clay body and a glaze 100% feldspar to achieve. Go figure. h a n s e n Link to comment Share on other sites More sharing options...
Teresita Posted June 28, 2010 Report Share Posted June 28, 2010 I have found that a slow bisque firing to cone 04 instead of cone 06 has been helpful Link to comment Share on other sites More sharing options...
nancirose Posted June 28, 2010 Report Share Posted June 28, 2010 I have gotten into the habit of spraying a light spray of water onto my bisqued pieces before glazing. Results =no more pin holes Link to comment Share on other sites More sharing options...
nancy Posted June 29, 2010 Report Share Posted June 29, 2010 I just dipped my pieces in my glaze and there were a lot of pin holes, so I rinsed off the glaze. Do I need to re bisque fire my piece before I try to glaze it again? The specific Gravity of the glaze is 1.45. Should it be thinner for dipping? Sharon no you do not have to rebisque your pots before glazing again. just wipe off the glaze with wet sponge or better still scrape off with a metal rib back into the glaze bucket-when completely dry to touch (doesn't feel cool) you may reglaze. Link to comment Share on other sites More sharing options...
Marcia Selsor Posted July 4, 2010 Report Share Posted July 4, 2010 I just dipped my pieces in my glaze and there were a lot of pin holes, so I rinsed off the glaze. Do I need to re bisque fire my piece before I try to glaze it again? The specific Gravity of the glaze is 1.45. Should it be thinner for dipping? Sharon Sherman gives good advice. Also after the glaze dries, use a dry finger to rub the pinholes smooth. Link to comment Share on other sites More sharing options...