Jump to content


Photo
- - - - -

Kiln shelf repair


  • Please log in to reply
7 replies to this topic

#1 Diane Puckett

Diane Puckett

    Advanced Member

  • Members
  • PipPipPip
  • 398 posts
  • LocationAsheville, NC

Posted 25 April 2013 - 01:39 PM

Two of my test glazes ran onto a kiln shelf. I swear the glazes ate partially through the shelf. I know I have to grind out all the glaze. This is leaving a gouge in the shelf. Is there something I can use to permanently fill that area before decorating with kiln wash?
Diane Puckett
Dry Ridge Pottery

#2 gypsy

gypsy

    Advanced Member

  • Members
  • PipPipPip
  • 89 posts
  • LocationJames Creek, Pa

Posted 25 April 2013 - 01:43 PM

Two of my test glazes ran onto a kiln shelf. I swear the glazes ate partially through the shelf. I know I have to grind out all the glaze. This is leaving a gouge in the shelf. Is there something I can use to permanently fill that area before decorating with kiln wash?


You know I have the same problem...pitted kiln shelves...I'm thinking kiln cement might work but am anxious to hear what others think about this too.

#3 neilestrick

neilestrick

    Neil Estrick

  • Members
  • PipPipPip
  • 4,904 posts
  • LocationGrayslake, IL

Posted 25 April 2013 - 02:09 PM

Just fill the hole with extra kiln wash.

Neil Estrick
Kiln Repair Tech
L&L Kilns Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

[email protected]


#4 Frankiegirl

Frankiegirl

    Advanced Member

  • Members
  • PipPipPip
  • 39 posts
  • LocationFL

Posted 25 April 2013 - 03:07 PM

Just fill the hole with extra kiln wash.



This is what I have always done. Works great for me and I have had more than my fair share of kilncidents

#5 perkolator

perkolator

    Advanced Member

  • Members
  • PipPipPip
  • 435 posts
  • LocationCalifornia

Posted 25 April 2013 - 04:12 PM

just wash right over it. if the shelf gets really bad after repeat cleanups, simply buy another shelf and keep the old one as a "waste shelf" that you don't mind messing up. standard kiln shelves are pretty cheap IMO when you compare it to the high-tech ones out now.

i always make students test glazes in a pre-fired firing tray or saggar simply to avoid this exact problem.

#6 Diane Puckett

Diane Puckett

    Advanced Member

  • Members
  • PipPipPip
  • 398 posts
  • LocationAsheville, NC

Posted 25 April 2013 - 04:16 PM

Thanks, everyone. This was a kiln full of glaze tests. I guess I need to make shelves just for this purpose.
Diane Puckett
Dry Ridge Pottery

#7 neilestrick

neilestrick

    Neil Estrick

  • Members
  • PipPipPip
  • 4,904 posts
  • LocationGrayslake, IL

Posted 25 April 2013 - 04:25 PM

If it's just test tiles, roll out a slab, coat it with kiln wash, and set the tiles on it.

Neil Estrick
Kiln Repair Tech
L&L Kilns Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

[email protected]


#8 Mark C.

Mark C.

    Advanced Member

  • Members
  • PipPipPip
  • 6,121 posts
  • LocationNear Arcata Ca-redwood rain forest

Posted 18 May 2013 - 02:18 AM

You could also fill it with the special ITC filler and wash over it . This stuff is spendy but works great.
Mark
Mark Cortright
www.liscomhillpottery.com




0 user(s) are reading this topic