Jump to content
Sign in to follow this  
GA_Clayman67

Cracking Prevention

Recommended Posts

Back into the clay after 37-years away and I'm having what has to be a simple problem, but I'm flummoxed!

 

Making very basic business card holders from slabs. I'm draping the cut piece of clay over a plastic covered 2x4 and letting it sit for 24-hours - also covered. Then, removing the plastic and allowing the pieces to dry on the 2x4.

 

My problem: nearly all the pieces are cracked after the second day and unusable.

 

What can I do to prevent this?

 

Many thanks in advance!

 

Art Carlson

Share this post


Link to post
Share on other sites

Or you could work within a negative right angle. When using wood forms, try sprinkling bal clay or corn starch on the surface to eliminate the clay from sticking to a rigid form. I use newsprint paper between clay and forms when necessary. The link is definitely overkill for business card size, but you will get the idea.

 

 

http://ceramicartsdaily.org/clay-tools/making-clay-tools/the-right-angle-for-approaching-geometric-ceramic-sculpture/

 

Marcia

Share this post


Link to post
Share on other sites

Or you could work within a negative right angle. When using wood forms, try sprinkling bal clay or corn starch on the surface to eliminate the clay from sticking to a rigid form. I use newsprint paper between clay and forms when necessary. The link is definitely overkill for business card size, but you will get the idea.

 

 

http://ceramicartsda...amic-sculpture/

 

Marcia

 

 

Thank you! I like the idea of corn starch - will try that next time around.

Share this post


Link to post
Share on other sites

IF you're draping around two corners, it won't work because the clay is shrinking as it dries and the board is not. If just around one corner, you could get away with putting something between the form and the clay so its not stuck to the form as it dries. My current go-to favorite is an old paper towel, but if I'm drying slowly a piece of saran wrap works just fine as long as I cover both sides

Share this post


Link to post
Share on other sites

IF you're draping around two corners, it won't work because the clay is shrinking as it dries and the board is not. If just around one corner, you could get away with putting something between the form and the clay so its not stuck to the form as it dries. My current go-to favorite is an old paper towel, but if I'm drying slowly a piece of saran wrap works just fine as long as I cover both sides

 

 

 

Maryjane...

 

thanks... Saran Wrap's a real pain - delighted to hear a paper towel works as well!

Share this post


Link to post
Share on other sites

Yep, just be sure to get CHEAP paper towels... I ran into some of the spendy ones that have some sort of softener in the paper that actually left marks on the fired piece. VERY strange, almost like a series of very fine wax resist dots anywhere they were in contact with the clay, even after the bisque. Would have been great if that was what I was looking for, but they wouldn't take the terra sig I was TRYING to apply.

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!