I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

Share this post


Link to post
Share on other sites

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

The reports I have heard about this glaze, and most iron reds and tomato reds, you fire to temp, hold, ramp it down, or whatever you do, then before it goes cold, refire to cone 05

h a n s e n

 

 

 

Share this post


Link to post
Share on other sites

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

 

I agree. Holding the temperature even only for 20 minutes at ^6 and again at 1825 will make a big difference. Also muddy color is when it is a little thick. This is a touchy glaze. A thin but not too thin coat really goes red. One of my kilns has a cone setter. I just push the button back on and hold it at the high temp. for 20 minutes and let it drop. Then turn it back on again at 1825. If I miss it, I just turn it back on and take it up to that temperature and hold. I haven't held it for more than 30 minutes.

Share this post


Link to post
Share on other sites

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

 

I agree. Holding the temperature even only for 20 minutes at ^6 and again at 1825 will make a big difference. Also muddy color is when it is a little thick. This is a touchy glaze. A thin but not too thin coat really goes red. One of my kilns has a cone setter. I just push the button back on and hold it at the high temp. for 20 minutes and let it drop. Then turn it back on again at 1825. If I miss it, I just turn it back on and take it up to that temperature and hold. I haven't held it for more than 30 minutes.

 

 

What happens in iron red glazes is that unless "bumped" or re-fired they come out brown. Because the cooling is too fast for iron to form the red coloration on the surface of the pot. Sometimes adding more bone ash in these glazes helps, so i am told. Does this help? The way it was first told to me is to cool it to very dull red then bump it back to cherry red, but nowadays we don't look into the kilns which is a unsafe practice, do we?

 

 

 

Share this post


Link to post
Share on other sites

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

 

I mix glazes for a local art center and just recently discovered that if you use Special red iron oxide (much redder and much more expensive) the Randy's will be red, sometimes tomato red with blacks and blues. For years we only got browns until I changed the RIO. No need to worry about holding, etc. as we fire 3 different kilns, all to cone 6. Results vary by kiln but all come out red.

Share this post


Link to post
Share on other sites

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

 

I agree. Holding the temperature even only for 20 minutes at ^6 and again at 1825 will make a big difference. Also muddy color is when it is a little thick. This is a touchy glaze. A thin but not too thin coat really goes red. One of my kilns has a cone setter. I just push the button back on and hold it at the high temp. for 20 minutes and let it drop. Then turn it back on again at 1825. If I miss it, I just turn it back on and take it up to that temperature and hold. I haven't held it for more than 30 minutes.

 

 

What happens in iron red glazes is that unless "bumped" or re-fired they come out brown. Because the cooling is too fast for iron to form the red coloration on the surface of the pot. Sometimes adding more bone ash in these glazes helps, so i am told. Does this help? The way it was first told to me is to cool it to very dull red then bump it back to cherry red, but nowadays we don't look into the kilns which is a unsafe practice, do we?

 

 

 

I am using a slightly different ^6 oxidation red from Michael Bailey's book.

I don't refire to ^05., I just hold the kiln at ^6 then again at 1825. If I miss that temperature as it is dropping, I turn the kiln back on, say..at 1700, and take it back up to 1825 and hold for 20-30 minutes. I am getting nice reds. But, if the glaze is on just a little thick, it will go brown.

Marina likes this

Share this post


Link to post
Share on other sites

yeah and if your recipe has bone ash sometimes increasing the bone ash is known to make red redder

 

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

 

I agree. Holding the temperature even only for 20 minutes at ^6 and again at 1825 will make a big difference. Also muddy color is when it is a little thick. This is a touchy glaze. A thin but not too thin coat really goes red. One of my kilns has a cone setter. I just push the button back on and hold it at the high temp. for 20 minutes and let it drop. Then turn it back on again at 1825. If I miss it, I just turn it back on and take it up to that temperature and hold. I haven't held it for more than 30 minutes.

 

 

What happens in iron red glazes is that unless "bumped" or re-fired they come out brown. Because the cooling is too fast for iron to form the red coloration on the surface of the pot. Sometimes adding more bone ash in these glazes helps, so i am told. Does this help? The way it was first told to me is to cool it to very dull red then bump it back to cherry red, but nowadays we don't look into the kilns which is a unsafe practice, do we?

 

 

 

I am using a slightly different ^6 oxidation red from Michael Bailey's book.

I don't refire to ^05., I just hold the kiln at ^6 then again at 1825. If I miss that temperature as it is dropping, I turn the kiln back on, say..at 1700, and take it back up to 1825 and hold for 20-30 minutes. I am getting nice reds. But, if the glaze is on just a little thick, it will go brown.

 

 

 

 

Share this post


Link to post
Share on other sites

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

 

I mix glazes for a local art center and just recently discovered that if you use Special red iron oxide (much redder and much more expensive) the Randy's will be red, sometimes tomato red with blacks and blues. For years we only got browns until I changed the RIO. No need to worry about holding, etc. as we fire 3 different kilns, all to cone 6. Results vary by kiln but all come out red.

 

 

What kind of RIO are you using that is so much redder than RIO that isn't so red? Crocus Martis is purplish. Spanish red iron oxide is fine red. Could you specify what it is you are using? I have three RIOs in my studio, plus Black Iron Oxide.

Inquiring minds want to know.

Thanks.

Share this post


Link to post
Share on other sites

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

 

I mix glazes for a local art center and just recently discovered that if you use Special red iron oxide (much redder and much more expensive) the Randy's will be red, sometimes tomato red with blacks and blues. For years we only got browns until I changed the RIO. No need to worry about holding, etc. as we fire 3 different kilns, all to cone 6. Results vary by kiln but all come out red.

 

 

What kind of RIO are you using that is so much redder than RIO that isn't so red? Crocus Martis is purplish. Spanish red iron oxide is fine red. Could you specify what it is you are using? I have three RIOs in my studio, plus Black Iron Oxide.

Inquiring minds want to know.

Thanks.

 

 

The redder RIO is called SPECIAL and we order from Ceramic Supply of New York and New Jersey (http://www.7ceramic.com/). You can call them and ask what makes it different but my guess is taht it is purer. (Ceramic Supply Inc, 7 Route 46 West, Lodi, NJ 07644, 973.340.3005, 800-723-7264). They are owned by Standard Clay in PA.

 

Special RIO costs much more than regular Spanish RIO. Eg 5 lb of Special is $13.50 and 5 lb vs 5 lb Spanish at $4.05. We use that cheaper Spanish RIO in glazes like Ron Roy Black #3 and Floating Blue (makes better blues). Overall, Special makes a redder cast in glazes but strangely makes the Floating Blue flatter, with green highlights in it more than blue. It's actually nice but students at the art center want BLUE.

 

Another tip, Dark Rutile works much better in Floating Blue than Light Rutile. Lt Rutile made the FB whiter and sort of flat looking. My guess is that less pure ingredients in FB make more textures in the melt. More pure will flatten it out.

 

Additionally, Special RIO will also make your red brown slips stay redder vs going dark brown at cone 6. Not sure what happens at Cone 10 gas reduction firings as never used it for our cone 10 glazes. I suspect that the higher temp and reduction will brown it out anyway so no reason to use something that costs 3x as much for the same effect.

 

Have not tried crocus martis as it is even MORE expensive than the Special. Hope that helps answer your questions.

Share this post


Link to post
Share on other sites

I have mixed a batch of Randy's Red - Cone 5 Glaze. I am getting more of a muddy brown than reddish brown. If anyone has used this common recipe - do you have any thoughts on how to adjust recipe to get the "red' back.

 

 

I mix glazes for a local art center and just recently discovered that if you use Special red iron oxide (much redder and much more expensive) the Randy's will be red, sometimes tomato red with blacks and blues. For years we only got browns until I changed the RIO. No need to worry about holding, etc. as we fire 3 different kilns, all to cone 6. Results vary by kiln but all come out red.

 

 

What kind of RIO are you using that is so much redder than RIO that isn't so red? Crocus Martis is purplish. Spanish red iron oxide is fine red. Could you specify what it is you are using? I have three RIOs in my studio, plus Black Iron Oxide.

Inquiring minds want to know.

Thanks.

 

 

The redder RIO is called SPECIAL and we order from Ceramic Supply of New York and New Jersey (http://www.7ceramic.com/). You can call them and ask what makes it different but my guess is taht it is purer. (Ceramic Supply Inc, 7 Route 46 West, Lodi, NJ 07644, 973.340.3005, 800-723-7264). They are owned by Standard Clay in PA.

 

Special RIO costs much more than regular Spanish RIO. Eg 5 lb of Special is $13.50 and 5 lb vs 5 lb Spanish at $4.05. We use that cheaper Spanish RIO in glazes like Ron Roy Black #3 and Floating Blue (makes better blues). Overall, Special makes a redder cast in glazes but strangely makes the Floating Blue flatter, with green highlights in it more than blue. It's actually nice but students at the art center want BLUE.

 

Another tip, Dark Rutile works much better in Floating Blue than Light Rutile. Lt Rutile made the FB whiter and sort of flat looking. My guess is that less pure ingredients in FB make more textures in the melt. More pure will flatten it out.

 

Additionally, Special RIO will also make your red brown slips stay redder vs going dark brown at cone 6. Not sure what happens at Cone 10 gas reduction firings as never used it for our cone 10 glazes. I suspect that the higher temp and reduction will brown it out anyway so no reason to use something that costs 3x as much for the same effect.

 

Have not tried crocus martis as it is even MORE expensive than the Special. Hope that helps answer your questions.

 

Thanks.

I have three RIO in my studio plus a little crocus martis, plus Black iron oxide.

I'll have to do some tests and see if one works better than another. Thanks for your explanantion.

 

 

 

 

Share this post


Link to post
Share on other sites

This is a view of Michael Bailey's Iron Red fired to ^6 Ox. and held at about 1950 for 30 minutes.

http://ceramicartsdaily.org/community/index.php?app=gallery&module=images&section=viewimage&img=682

Take a good look at the bottom glaze on the mug. It is a nice iron red.

Marcia

Share this post


Link to post
Share on other sites

This is a view of Michael Bailey's Iron Red fired to ^6 Ox. and held at about 1950 for 30 minutes.

http://ceramicartsda...ewimage&img=682

Take a good look at the bottom glaze on the mug. It is a nice iron red.

Marcia

 

 

I used a commercial Iron Red for years at the HS. It was from Minnesota Clay. It was very thickness dependent. If you got it on thin it was a gloss brown black, thicker it became red with light speckling of olive green, thicker yet it got more olive greens in it but still stayed red. It was one of my favorite glazes as once we got used to it- it was always successful.

Share this post


Link to post
Share on other sites

This is a view of Michael Bailey's Iron Red fired to ^6 Ox. and held at about 1950 for 30 minutes.

http://ceramicartsda...ewimage&img=682

Take a good look at the bottom glaze on the mug. It is a nice iron red.

Marcia

 

 

I used a commercial Iron Red for years at the HS. It was from Minnesota Clay. It was very thickness dependent. If you got it on thin it was a gloss brown black, thicker it became red with light speckling of olive green, thicker yet it got more olive greens in it but still stayed red. It was one of my favorite glazes as once we got used to it- it was always successful.

 

 

 

 

Hi, I would love to have a good Randy's Red recipe if anyone would care to contribute one. :-)

 

thx,

Catsandgoddess@gmail.com

Share this post


Link to post
Share on other sites

Just found my Randy's Red formula we use in the art center. Very different from the other one I sent you earlier. We fire in Tucker's ConeArt kiln with 3 inch thick walls. Fires hotter than we like as will cause running at Cone 6 (by their electronic controller), so knocked back Cone 6 temp by 30 degrees. Cools very slowly. When same glaze is fired in older kilnsitter kiln, glaze will be browner definitely. Can try refiring to bisque Cone 06 but that doesn't always work. I think hotter is better and Cone 5 just isn't hot enough.

 

 

Percent

24 Flint/Silica

4 EPK

8 Soda Ash

25.6 Gerstley Borate

16 F4 SPAR

14 TALC

12.12 RIO

1 Bentonite

 

 

FYI Adds up over 100.

 

Different formula, not tested but note that must fire hot.[Randy’s Red (in grams) Low Cone 7 or hot Cone 6Flint 75.00 grams

 

EPK 12.50

 

F-4 spar 50.00

 

Talc 35.00

 

Gerstley Borate 80.00

 

252.50 grams

 

+RIO 37.80 (this is 15%)

 

(red iron oxide)

 

 

 

canyon fox has sent you this email from
.

 

 

Hi Jennie,

thank you for sharing about SPECIAL red iron oxide.

I ordered one and tried with two recipes I have and still got just muddy brown, almost black. Would you share your "reddest" recipe please? I fire to cone 5.

Thank you,

Lena

 

---------------------------------------------------

Share this post


Link to post
Share on other sites

Just found my Randy's Red formula we use in the art center. Very different from the other one I sent you earlier. We fire in Tucker's ConeArt kiln with 3 inch thick walls. Fires hotter than we like as will cause running at Cone 6 (by their electronic controller), so knocked back Cone 6 temp by 30 degrees. Cools very slowly. When same glaze is fired in older kilnsitter kiln, glaze will be browner definitely. Can try refiring to bisque Cone 06 but that doesn't always work. I think hotter is better and Cone 5 just isn't hot enough.

 

 

Percent

24 Flint/Silica

4 EPK

8 Soda Ash

25.6 Gerstley Borate

16 F4 SPAR

14 TALC

12.12 RIO

1 Bentonite

 

 

FYI Adds up over 100.

 

Different formula, not tested but note that must fire hot.[Randy’s Red (in grams) Low Cone 7 or hot Cone 6Flint 75.00 grams

 

EPK 12.50

 

F-4 spar 50.00

 

Talc 35.00

 

Gerstley Borate 80.00

 

252.50 grams

 

+RIO 37.80 (this is 15%)

 

(red iron oxide)

 

 

 

canyon fox has sent you this email from
.

 

 

Hi Jennie,

thank you for sharing about SPECIAL red iron oxide.

I ordered one and tried with two recipes I have and still got just muddy brown, almost black. Would you share your "reddest" recipe please? I fire to cone 5.

Thank you,

Lena

 

---------------------------------------------------

 

 

Try this link to see the difference in iron reds with and without cooling cycle. There are formulas and the firing cycle given. http://wpapotters.blogspot.com/2011/10/cone-6-oxidation-results-group-5.html

Share this post


Link to post
Share on other sites

Michael Bailey's recipe

I always understood here was a need for bone ash in Iron reds. I don't see that in some of the opted recipes.

But if it works then great. In Michael Bailey's cone 6 Oxidation book he provides many variation with additions from 0 up to 23% red Iron Oxide with the color transitions from

white through yellow , tan brown speckled, with the brightest reds in the 11%-18% range. Here is the recipe:

Bailey's Orange red Base Glaze

Potash Feldspar 46.7

Kaolin 4

Bentonite 2

Bone Ash 15

Lithium Carb. 4

Talc 16.9

Silica 11.4

total 100.0

 

Red Iron Oxide 11.5%

 

I soak it at ^6 for about 20 minutes and drop to 1900 for 30 minutes soak. see on the bottom of mug here

chttp://ceramicartsda...ewimage&img=682

Share this post


Link to post
Share on other sites

Michael Bailey's recipe

I always understood here was a need for bone ash in Iron reds. I don't see that in some of the opted recipes.

But if it works then great. In Michael Bailey's cone 6 Oxidation book he provides many variation with additions from 0 up to 23% red Iron Oxide with the color transitions from

white through yellow , tan brown speckled, with the brightest reds in the 11%-18% range. Here is the recipe:

Bailey's Orange red Base Glaze

Potash Feldspar 46.7

Kaolin 4

Bentonite 2

Bone Ash 15

Lithium Carb. 4

Talc 16.9

Silica 11.4

total 100.0

 

Red Iron Oxide 11.5%

 

I soak it at ^6 for about 20 minutes and drop to 1900 for 30 minutes soak. see on the bottom of mug here

chttp://ceramicartsda...ewimage&img=682

 

Thank you for sharing the recipe, Marcia.

It's hard to see, is your red matte or glossy?

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×

Important Information

By using this site, you agree to our Terms of Use.