Ray Bright Posted October 10, 2012 Report Share Posted October 10, 2012 My 1st firing has produced a strange effect: the clear glaze on the edges of my pieces are smooth, but in the center they are bumpy, seem not totally fixed to the substrate, covered with a sort of orange peel. The glaze is still clear, not all pieces are like this, and I think I may have laid on way too much glaze in my zeal to make very shinny objects. Humm? Link to comment Share on other sites More sharing options...
neilestrick Posted October 10, 2012 Report Share Posted October 10, 2012 Possibly too thick, underfired, or crawling. Is this a glaze you've used before? Link to comment Share on other sites More sharing options...
Ray Bright Posted October 11, 2012 Author Report Share Posted October 11, 2012 Possibly too thick, underfired, or crawling. Is this a glaze you've used before? No. AMACO LG-10. I think I laid it on too thick. Within the same piece, the glaze is good & bumpy. So it fired properly. Where it's bumpy, is where I glopped on a big dab of glaze (3 times) which I then spread out toward the edges, which are just fine. Three days ago I fired a kiln for the first time in my life. I'm making it up as I go along, knowing nothing. I'm a retired movie producer whose fallen in love with the ceramic process. (my father was bricklayer). I'm very used to winging it, with far more pressure than this calls for. But I'm in it to make the thing I want to make as good as it can be made. Thanks, Ray Link to comment Share on other sites More sharing options...
neilestrick Posted October 11, 2012 Report Share Posted October 11, 2012 LG-10 is typically very consistent, so you must have applied it too thickly. Link to comment Share on other sites More sharing options...
Ray Bright Posted October 11, 2012 Author Report Share Posted October 11, 2012 LG-10 is typically very consistent, so you must have applied it too thickly. I really laid it on. Next test this Friday, think thin. Link to comment Share on other sites More sharing options...
neilestrick Posted October 11, 2012 Report Share Posted October 11, 2012 Although the labels usually say 3 coats, you can often get by with 2 flowing coats, brushed on in opposite directions. Depends on how thick they mixed it. Link to comment Share on other sites More sharing options...
Lucille Oka Posted October 12, 2012 Report Share Posted October 12, 2012 To what cone or temperature did you fire this LG-10 glazed ware? Link to comment Share on other sites More sharing options...
ayjay Posted October 12, 2012 Report Share Posted October 12, 2012 Although the labels usually say 3 coats, you can often get by with 2 flowing coats, brushed on in opposite directions. Depends on how thick they mixed it. The brush can make a difference too, I find a soft fan brush is good for glazes designed to be brushed on but I use something that holds a lot more glaze if I'm brushing on a dipping glaze. Link to comment Share on other sites More sharing options...
Ray Bright Posted October 12, 2012 Author Report Share Posted October 12, 2012 To what cone or temperature did you fire this LG-10 glazed ware? Fired to cone 05. Using very old Skutt with bar type cone in Kiln sitter. Some things on the most problematic shelf came out perfect, but these had much more vertical surface. The orange peeling ones were 95% flat, and I think I put so much glaze on it pooled in the middle and couldn't finish properly. This was my 1st firing/test of this system, will no much more soon. Will use only 2 coats with same application method. R Link to comment Share on other sites More sharing options...
Lucille Oka Posted October 14, 2012 Report Share Posted October 14, 2012 I am trying to understand the term you used 'orange peel'. If there are a lot of 'teeny tiny pits' (orange peel) this is a bit of a thin application and an underfire. If you see a lot of small bubbles under the glaze surface and those bubbles make the glaze look a bit cloudy then yes you applied too much glaze. Link to comment Share on other sites More sharing options...