A midfire Shino I recently mixed up is misbehaving. Dipped pots are emerging from the glaze covered with air bubbles. I have a leftover bit of the same formula that covers just fine. I mix the glaze very gently, so I'm pretty sure I am not causing it by stirring air into the glaze.

And any other glaze over the Shino will also be pitted with air bubbles, although the second glaze will cover perfectly elsewhere on the same pot...

Worst of all, I'm embarrassed to admit that this same thing happened to me last year, but I'll be damned if I can remember the cause or solution.

Could someone help this dunderhead?

Link to comment
Share on other sites

Does your shino have soda ash in it? I want to recall that soda ash, when stirred, can create the air bubbles in the glaze. (Remember, the soda ash migrates to the surface of the pot to form those really cool crystal fuzzy thingies for carbon trapping.) They will go away if you allow some time between stirring and dipping. Or you can use a strainer to skim the surface of the glaze to remove the air bubbles. I think soda ash loses its potency over time, which might explain why your older shino does not have the problem.

Link to comment
Share on other sites

I mix the glaze very gently, so I'm pretty sure I am not causing it by stirring air into the glaze.

 

Unless the glaze looks like foamy head of a freshly poured pint of bitter... you are fine.

 

Dipped pots are emerging from the glaze covered with air bubbles.

Is your glaze too thick or you put it on too thick?

Use your finger to smooth out those bubble craters on the bisque and you will be fine.

 

Any chance you can upload a small image of that bubbling glaze?

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.