Min Posted September 7, 2018 Report Share Posted September 7, 2018 Mary, could you post your original Old Gold Albany recipe that you are subbing Hudson clay in? As adding just 5% feldspar isn't enough I would try a progression blend, adding 5 grams at a time and going up to 25grams per 100 base. Try banging the edges of the un-shivered test tiles against something hard, might see more shivering. Shivering can happen straight away or years later, don't trust a glaze that shivers. Link to comment Share on other sites More sharing options...
GreyBird Posted September 7, 2018 Author Report Share Posted September 7, 2018 Sure, Old Gold Albany: Albany Slip: 78% Lithium Carb: 10% Zircopax: 12% No, I don't trust it at all. That is why I am trying to adjust it to be a trustworthy stable glaze Link to comment Share on other sites More sharing options...
Magnolia Mud Research Posted September 7, 2018 Report Share Posted September 7, 2018 Drop the lithium carb and see what happens. or swap sodium or potassium carbonate for the lithium carb. LT Link to comment Share on other sites More sharing options...
GreyBird Posted September 7, 2018 Author Report Share Posted September 7, 2018 I'll try that. If I just drop the Lithium Carb the recipe won't add up to 100% does that matter? If it works I guess I would just adjust it to add up to 100% and go with that? Link to comment Share on other sites More sharing options...
Magnolia Mud Research Posted September 7, 2018 Report Share Posted September 7, 2018 Your logic is sound. tweaking is easier working with the 'original' mixture . Renormalize to 100% after you have what you want. Link to comment Share on other sites More sharing options...
Min Posted September 7, 2018 Report Share Posted September 7, 2018 There's an Alberta Slip ^6 glaze that is based on that Albany Slip one but with a higher COE to address the shivering that used to come with that glaze. Uses 21% 3195 and drops the lithium carb to 5. https://digitalfire.com/4sight/recipes/alberta_slip_lithium_brown_cone_6_35.html Link to comment Share on other sites More sharing options...
GreyBird Posted September 7, 2018 Author Report Share Posted September 7, 2018 Thank You!!! Link to comment Share on other sites More sharing options...
glazenerd Posted September 7, 2018 Report Share Posted September 7, 2018 Mary: your recipe is 78% clay, 10% strong flux to melt the 78% clay, and 12% colorant to change the color of the 78% clay. So it still comes back to the clay; so I will break it down : Albany: total fluxes 16.97%. Alumina. 10.51%. Iron 2.11% Silica 70.40%. ( molar %) Hudson:total fluxes 13.41% Alumina. 13.52%. Iron 3.71%. Silica. 68.54%. (Molar %) So in formulating: Albany has more total fluxes, so it needs less flux additions to melt- Hudson needs more. Hudson has a third more alumina and less silica than Albany which throws off the SiAl ratio. Did you notice in the recipe Min posted: the 5% alumina hydrate addition? That was done to balance the SiAl ratio, to bring it into limits. Alumina adds strength to clay, just as it does glaze. Finally, Albany has 2.11% iron and Hudson 3.71%. When firing to cone six: iron has to be factored in as additional flux. It is this same iron level variation playing into the color: with some minor contributions elsewhere. I would shy away from any sodium additions due to the clay content of the recipe: pin hole issues are probable. Potassium would be a good alternate choice. Hudson already has a high calcium content: no need to add that either. Montmorillonite based clays are very plastic, but also very weak. In your case, prone to shivering. You could also use your original recipe and add 5% alumina hydrate to that. Another variation: add 10% EPK ( kaolin is 37% alumina). The primary distinction being: you are melting a recipe with 78% clay content. T forgot something: the high level of iron in Hudson could also be playing a role in this problem. High iron content in clay can make it brittle. Link to comment Share on other sites More sharing options...
GreyBird Posted September 8, 2018 Author Report Share Posted September 8, 2018 Glazenerd, Thank you so much for taking the time to go into this so thoroughly. I feel rather inadequate when it comes to chemistry but I am hoping the glaze class will give me a bit of a boost! Link to comment Share on other sites More sharing options...
mousey Posted September 8, 2018 Report Share Posted September 8, 2018 On 9/4/2018 at 7:58 PM, GreyBird said: Here is how it bisqued at 04: And this is why the Hudson Valley is famous for its brickworks Lotta old brick kilns out and about as well. Link to comment Share on other sites More sharing options...
GreyBird Posted September 8, 2018 Author Report Share Posted September 8, 2018 OK, I am going to mix these two up tomorrow and see how it goes New Old Gold Albany:Albany Slip - 75 Frit 3195 - 20 Alumina Hydrate - 5 Tin ox - 4 New Old Gold Hudson:Hudson Clay - 75 Frit 3195 - 15 EPK - 15 Tin ox - 4 The original had 12% Zircopax. Is there a reason to switch to tin and to lower it to 4%? I really liked the original "Old Gold" Color. I guess I could always try it both ways. I also found these in "Ceramic Glazemaking" by Richard Behrens. I'll try them as is before making adjustments for shivering Bright Matt Albany: Lithium Carb 00.9 Zinc ox 09.8 Kaolin 05.2 Albany Slip 84.1 Bright Mottled Albany: Lithium Carb 14.8 Albany Slip 74.2 Kaolin 11.0 Bentonite 02.0 Link to comment Share on other sites More sharing options...
glazenerd Posted September 9, 2018 Report Share Posted September 9, 2018 Mary: Want to see your clay up close? You can see the alkali film bleeding across the sedimentation lines in the first pic. In the second pic which is towards the surface: looks like the high iron content is oxidizing. You definitely have a large amount of mica: can see the crystals in other views. Which explains the high potassium and higher alumina levels. I did an "unofficial" sieve test yesterday: I sieved about 1/4 pound through a 100 mesh screen. Then I took one level teaspoon and sieved through a 200 mesh screen: about 70% passed. Unofficial, but gives me some indication of what you are dealing with. I can also see a green cast in some views: usually associated with chlorite minerals. Early in the game at this point: but I am going with some smectite variety, which has heavy mica deposits, hematite, and ??? (will have to test more). What I was wrong about: little to no humus. Been awhile since I have seen natural clay bleed fluxes. Suspect this is your iron (8.31%) oxidizing as it is exposed to air. Tom Link to comment Share on other sites More sharing options...
GreyBird Posted September 9, 2018 Author Report Share Posted September 9, 2018 WOW, Cool Pics. So interesting. Thanks for sharing though without your narration I wouldn't have a clue as to what I was looking at. LOL. I know that someone else who had done some experimental firing with it had said he had an issue with salt migrating to the surface. Could that be salt in the top pic? Link to comment Share on other sites More sharing options...
glazenerd Posted September 9, 2018 Report Share Posted September 9, 2018 Both potassium and sodium are naturally occurring salts. In both cases, they can contain 14-20% soluble salts; which indeed migrate. Still makes me wonder if a water treatment plant is dumping upstream? Very unusual. Maybe you should call it "Calgon Hudson Clay" Tom Will have a test fire out later today: will post later. Link to comment Share on other sites More sharing options...
glazenerd Posted September 9, 2018 Report Share Posted September 9, 2018 Cone 6. 60% Hudson, 20% spodumene, 20% mahavir potash, 3% NS suspender, 3% lithium. Carb. so far so good: going to thermal shock when I get time. Just slightly immature, but close. I see red streaks sprinkled throughout. Going to try 50%, which should go red! then 70%. The recipe brings silica just over limits, but the alumina is way heavy ( intentionally). Link to comment Share on other sites More sharing options...
GreyBird Posted September 9, 2018 Author Report Share Posted September 9, 2018 Cool.. Looking forward to your results! Link to comment Share on other sites More sharing options...
glazenerd Posted September 14, 2018 Report Share Posted September 14, 2018 Mary: been doing some research, trying to figure out your clay. calcium bentonite is found in your area. Calcite is mined and abundant all over NY state. More interesting, smecite is fairly common in the Arirondack Mts. Even more interesting is how it is formed: humus is drawn into existing illite deposits on the forest floor and is converted over (much) time to a smecite variety. Even more interesting, native NY smecite has a green/ gray cast: which I saw in your samples. The specific native NY smecite is 0.5 um particle size: in pottery speak 2500 mesh plus. Question: how far away is Cherry Hills? And it's proximity to the Hudson? Tom Link to comment Share on other sites More sharing options...
GreyBird Posted September 14, 2018 Author Report Share Posted September 14, 2018 Is Cherry Hills town in NY State? I can't seam to locate it on Google.. Link to comment Share on other sites More sharing options...
glazenerd Posted September 14, 2018 Report Share Posted September 14, 2018 Mary: was reading several pieces on mineral resources found in NY: one referenced Cherry Hills. Might have read it wrong; might be an old mine? I could not find it either. Tom Link to comment Share on other sites More sharing options...
Gred Posted September 14, 2018 Report Share Posted September 14, 2018 Thanks so much for sharing all of this info. Quick question. What do you think contributes to the high iron levels? I ask because I believe that area of the Hudson was once a site of great oyster beds. I used to do some oyster work to help spawn oyster beds and I know oysters have a high iron content. Just wondering if anyone is aware if there is a correlation. Link to comment Share on other sites More sharing options...
glazenerd Posted September 14, 2018 Report Share Posted September 14, 2018 Gred: oyster shells would provide calcium, not sure what else? The iron and magnesium levels are the highest I have seen in natural clays: not sure what the contributing factors are, but working on it. I originally thought the iron was hematite due to the color, but from reading; magnetite is more common in NY. Later this year I will demineralization a sample and have a look. I am fairly confident it is a combination of calcium bentonite and smecite montrollites. The old Albany slip was classed as non-plastic; this sample is highly plastic- approaching macaloid in nature. Interesting indeed! Tom edit: I will look into the iron levels in oysters Link to comment Share on other sites More sharing options...
GreyBird Posted September 15, 2018 Author Report Share Posted September 15, 2018 I am loving all of this detail and Googling a bunch of new words. LOL. Today's word... "macaloid". Thank you so much for sharing all of this information Link to comment Share on other sites More sharing options...
glazenerd Posted September 15, 2018 Report Share Posted September 15, 2018 Think I found the cause of 8.31% iron content: https://thediggings.com/mines/usgs10296653 mostly magnetite mines along the Hudson. Link to comment Share on other sites More sharing options...
glazenerd Posted September 16, 2018 Report Share Posted September 16, 2018 Mary: calcium bentonite is also abundant along the Hudson. Magnetite (iron) will present itself dark grey to black in sedimentary deposits. Plenty of mica and calcite around the Hudson as well. When I was candling some of the material, got that musty aroma of humus as well, albeit very low %. At this point, my prime suspects in your Hudson River clay. arsenic is a normal by- product of natural oxidation/reduction of iron, especially magnetite. https://pubs.acs.org/doi/abs/10.1021/es702625e Tom Link to comment Share on other sites More sharing options...
glazenerd Posted September 16, 2018 Report Share Posted September 16, 2018 Both of these are 50% Hudson, 20% potash, 5% lithium, 20% silica. Added titanium to one of them. Did the job of melting, but the potassium created some pin hole issues. Will need a hold at peak. I took them out of the kiln at 350F, and plunked them into cold water- survived well enough. Link to comment Share on other sites More sharing options...