Oxidation Shino ^6

Alberta Slip ... 56.0

Gerstley Borate ... 18.7

Soda Feldspar ... 9.4

Silica ... 9.4

Lithium Carbonate ... 6.5

Zircopax ... 9.4

Tin Oxide ... 4.7

 

This one's pretty good. Fat and creamy where thick, orange where thin.

 