Hey world,

 

By how much shoud I multiply Linda Abuckle's majolica glaze recipie to make a 5 gallon bucket? Here is the recipie.

 

Thanks,

 

Darrel

 

Majolica Glaze

Cone 04 OxidationGlaze Material

PercentageFrit 3124 (Ferro)65.72%Kona F-4 Feldspar17.23Nepheline Syenite 6.24Edgar Plastic Kaolin10.81Total100.0%Add:Tin Oxide 5.00%Zircopax10.00Bentonite

 

2.00

 

 

Share this post


Link to post
Share on other sites
Marcia Selsor    1,301

Darrel,

This glaze contains 65.72% grit which is dense. You can mix 10,000 grams into a 5 gallon bucket.

This is not always true if you are using light fluffy chemicals. But that much grit makes it an easy fit.

Marcia

Linda Arbuckle's Majolica

Frit 3124 (Ferro)65.72%

Kona F-4 Feldspar17.23

Nepheline Syenite 6.24

Edgar Plastic Kaolin10.81

Total 100.0%

Add:Tin Oxide 5.00%

Zircopax10.00

Bentonite

<br style="color: rgb(28, 40, 55); font-family: arial, verdana, tahoma, sans-serif; font-size: 13px; line-height: 19px; background-color: rgb(250, 251, 252); ">2.00 <br style="color: rgb(28, 40, 55); font-family: arial, verdana, tahoma, sans-serif; font-size: 13px; line-height: 19px; background-color: rgb(250, 251, 252); ">

Share this post


Link to post
Share on other sites
perkolator    53

I got this fancy glaze batch size reference sticker from glazecal.com when I was at NCECA this past year. I like it because I always forget.

Of course the weight will vary according to what type of materials go in.

 

 

Sticker says:

 

 

"8,000g - 5gal container

3,000g - 2gal container

1,500g - 1gal container

500g - 1 quart container

 

Start with a batch size you know will fit into your container. Gradually increase for each glaze."

 

 

 

Share this post


Link to post
Share on other sites
Marcia Selsor    1,301

dear percolator,

 

I have used Arbuckle's glaze and it fits in

To five gallon buckets because Frit is a dense material.

So do several other majolica glazes using high Frit contents.

Ps. I have been going to NCECA since 1971, served on the board in the 1990s and know for a fact that

This glaze will fit 10,000 grams into a five gallon bucket. This does make a very full bucket but I mixed it for a tile glazing workshop so it was good to have a full bucket.

 

The sticker you are referring to is an OK and just OK rule of thumb with a few exceptions...dense Frits being one of them. On the other extreme, ash glazes or Magnesium carbonate glazes may not fit 6000 grams into a 5 gallon bucket because the material is the opposite of dense. The two other examples are light and fluffy. This changes their mass in a five gallon bucket. this has been discussed on this forum previously.

 

Marcia

Share this post


Link to post
Share on other sites
Marcia Selsor    1,301

Here is additional information from her web site. Your recipe is slightly different going into 2 decimals.

http://lindaarbuckle.com/handouts/majolica_handout2007.pdf

 

When preparing the surface , sand any blemish and wash the piece with diluted vinegar and water.

 

After applying the glaze, and after it dries, smooth out any thick spots or pin holes.

 

Watch her video online. There are several sites and one on CAD.

 

Marcia

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×