PotsbyChar Posted May 13, 2011 Report Share Posted May 13, 2011 Does anyone have a lowfire 04-06 aventurine glaze recipe that they would be willing to share? I have done quite a lot of searching on line and have not been very successful. Thanks so much in advance for your help. Link to comment Share on other sites More sharing options...
Marcia Selsor Posted May 14, 2011 Report Share Posted May 14, 2011 Anne Currier Water Blue ^06 Frit 3110 73 Gerstley Borate 7 Silica 10 Kaolin 7 Zinc 3 Copper Carb. 4 Try this one. Marcia Link to comment Share on other sites More sharing options...
PotsbyChar Posted May 17, 2011 Author Report Share Posted May 17, 2011 Anne Currier Water Blue ^06 Frit 3110 73 Gerstley Borate 7 Silica 10 Kaolin 7 Zinc 3 Copper Carb. 4 Try this one. Marcia Thank you so much Marcia...will give this a try. Link to comment Share on other sites More sharing options...