I’m so glad you posted those links, I’m hung up on exactly this as well. If decomposition happens at 320C, I would certainly not be having the issues I’m having because my high fluxed (read: high boron) glazes begin to melt at around 750-800C. The idea behind the zinc is to have them melt much later and more vigorously, at cone 05-06, but the exact amount depends on when the decomposition phase ends!
-
I don’t get pinholes in my later melting copper glazes, but I am getting them in my own earlier melting copper glazes. I need to be firing at exactly 1000°C, so I my idea is to incorporate a zinc to delay melting and give the copper an opportunity to finish off gassing. As a matter of curiosity, what temperature does copper typically finish its offgassing?
-
Non chrome based green stain in a zinc base
mr_glazy_man replied to mr_glazy_man's topic in Clay and Glaze Chemistry
@PeterH Copper Oxide gives me dark specks. The carbonate is much more finely milled and gives a more uniform colour @Min good to know. I might go the non cadmium green and mix it with black and a pinch of blue to get a more emerald green. I’m too scared of poisonous cadmium! -
Hi, A number of posts back I was talking about a beautiful 04 fluid melt glaze I created with FZ16 and 3110. Doing a line blend between Iron Oxide and Copper Carb in this base yields a lovely green, but I feel like it needs more punch. Increasing the amount of oxide colourant just causes more bubbles and glaze defects due to the amount of off gassing (I’m at 5% Copper already!) So, I’m thinking about cutting it with some green stain to reduce the LOI, increase the green saturation but still get that oxide depth we all know and love. Alas, I’m sure most of you now know where this is going - most green stains are chrome based, and chrome+zinc is…. well, brown ain’t green. Can anyone recommend a non-chrome based green stain? Another tact might be Green Iron Oxide, which though is not stain based, may dial up the saturation of green but I really haven’t found much info in this at all online. What do you all think?
-
@Min Never heard of Magma. Alas, just tried ordering it online and they don’t ship down under. Rats! Cold dunking wouldn’t be an option with our line, but maybe a cold blast of air right out of the kiln might work on a larger scale. I’ll be sure to post back here if I give it a go. Thank you again all.
-
Success! I am happy to say that because of all of your wonderful help, I have been able to get this glaze right. Hats off to @Min for the suggestion of blending 3110 with the base glaze. The end result is an absolutely marvellous turquoise that fires at exactly 1040c and without a single defect. And, completely and utterly leadfree. The only thing I need to really work out now is how to increase the crazing. I’m working on getting the exact proportions correct, but see below attached photo. Base on the left, 3110 on the right. You can see that the host really needs the fritted zinc (not raw zinc oxide) to delay melting, otherwise surface problems.
-
Me too. I'll give it a shot with a line blend with some Turquoise stain. If I'm not so bloody rigid and just fire my ware at 1000 for this particular base, it's basically problem solved. And, it's a magical finish. 40 degrees (celcius) is literally what is separating me from where I am now and Leadless-Copper Valhalla.
-
Hi all, Big update. Image attached of results. I have conducted line blends of the following base (Copper Carb - 5% is added to all by default) and fired to 1040. Fast cool. All glaze weights were measured to ensure even application across the tile and equal amounts between tiles. Base FZ-16 - 90% EPK - 10% ------------------------------------------ Column 1 (Biaxial): 3134 - 85% EPK - 15% Notes: Didn't notice any difference at all between the blends. Important to note that this was a double line blend, not 10% addition of 3134. Again, opacification around the edges of the test tile, which is what I was getting with the FZ-16 Base at 1040. ------------------------------------------ Column 2: +2.5% Additions of Wollastonite Notes: As we go up, opacification increased. This is a similiar result to the EPK. We conclude here the additions of calcium does not resist copper or zinc's opacification in this base. ------------------------------------------ Column 3: +2.5% Additions of Whiting Notes: Big blisters. Likely a result of the LOI of whiting. Again, opacification of the copper. ------------------------------------------ Column 4: +2.5% Additions of Strontium Carb Notes: I was curious what this would give me, even though Strontium Carb isn't an active flux at these low temperatures (unless in frit form, which I don't have). Interestingly enough, the strontium resisted the opacification but there are a score or mirco-bubbles under the surface. This is likely the later LOI of Strontium Carb. Overall, unsatisfactory finish. Well, after all that, no movement towards the goal of getting FZ-16 to melt at 1040 the way it does at 960 or even 1000. Any ideas? I might have a go at line blending with 3110 which is a lower boron and thus higher melting frit.
-
Ugh, amazing. I love this community. Thank you - that’s incredibly helpful. If you don’t mind me asking - is there a resource you pulled this from? I’d love to get my hands on it! In terms of the double variable test - this would be a biaxial, correct? In such a case, I will test with: A: FZ-16 90% EPK 10% Copper Carb - 5% B: 3134 - 80% FZ-16 - 10% EPK 10% Copper Carb - 5% Im hesitant to go 20% EPK again because of how thick it was last time with the FZ-16. I ended up using Tetrasodium Pyrophosphate and CMC to deflocculate, slow drying a little just to make it workable. I’m weary of adding too much extra water, because it’ll dilute my S.G and aiming for gram weights on the ware will mean a lot of glaze I don’t want. I might also try another test with my initial base recipe and 2% increments of wollastonite. However, the unwanted added silica in the wollastonite has me thinking that whiting - as bob suggested - might be preferable. Besides, the zinc and it’s late melt should give time for the calcium carb to off gas properly. Time will tell I suppose. Maybe I’ll do both. I can’t say, because I haven’t tested on any curved geometry - only test tiles. But the glossiness and ability to heal over defects absolutely rivals lead bisilicate, just as he said. This is why I’m so keen to get the temp up - if I can get it to 1040, I’m grinning. Sadly not, but this has me thinking that I might want to invest in one now.
-
@Min Ah, but it’s the beautiful oxide transparency that I want. Stains just don’t look the same i am using glaze calc, but without having limit guides for earthenware (every target formula seems to be for cone 6) it just feels like I’m shooting in the dark. For calcium, I was initially thinking Wollastonite, but you’re right, frit form would be better. 3134 has close to 20% calcium, so I could line blend with that. Would you have any other suggestions?
-
3134 and 3124 is another interesting avenue, for sure. I feel like that one, in addition to the magnesium based 3249, are both candidates to do line blends with (though the 3249 will have the opposite effect to crazing). The reason I test across the temperature range is to observe how a material behaves under different intensities of heat. It’s laborious, but enables me to visually distinguish symptoms of under and over firing. I’ll be playing with a number of other permutations of materials this week and I’ll post the update. Thank you for the compliments!
-
Unfortunately I’m at an odd’s end as to why the copper is opacifying at all - I haven’t been able to find anything on Digital Fire or other adjacent sites that suggest anything about copper opacification. @BobMagnuson provided a nice trail to follow with the suggestion that it might be the zinc opacifying, but it doesn’t explain the opacification in other hosts - which leads me to suspect that this is specifically related to the copper.
-
@Bill Kielb I fire the kiln at the ramp cycle recommendations set out in the Orton Self Supporting Cones chart to verify correct heat work and temperature. If I get the corresponding 90Degree bend, then my temperatures are correct Do you suspect an incorrect temperature that might be causing the copper’s opacification?
-
@BabsCone 05-04 is our standard range at the moment. All of our product gets fired between these cones. The FZ-16 base I have is melting beautifully at 09-08 (extraordinary really, and with no lead)! Ideally, I want everything firing at the same temperature range, which is why I’m interested in increasing this base’s temperature. Silica and EPK have not helped me in this respect.
-
Thanks for the responses team. @BobMagnuson I didn't know that Zinc opacifies sans calcium. Definitely a trail for me to explore. Note below the line blends I did. To clarify: First column: the recipe fired across the temp range. You can see that at 940C and 1000C, it fires absolutely magnificently (and this is with Copper Carb, which has given me nothing but problems blisters, orange peel surface in every other base glaze I've tested at the temperature) Second column: Line Blend adding 1% Silica. Zinc begins to opacify and thermal expansion is reduced Third column: Line Blend adding 1% EPK (on top of the 10% already present). Zinc begins to opacify almost immediately. This shocked me. Next test would be to proceed as @BobMagnuson suggested (but with Wollastonite given the LOI issues with whiting) and @Min suggestion of 3110. Would it just be the lack of calcium causing this opacification? It seems that the opacification is correlated with the copper as I'm getting opacification when put into other zinc free low fire high thermal expansion transparent bases. For example, see below triaxial test of 94% frit (3110, 3195 and 3134 in each corner), 6% EPK and 5% Copper Carb fired at 1040C
-
What material could I use to raise firing temperature of a crazing glaze? For the record, I like that it's crazing and want to preserve that. I am using copper as the colouring oxide to get a beautiful turquoise blue, and am noticing that it becomes opaque as we reach temperature (1040c)for this base glaze. I am presuming that the copper is therefore overfiring in the base glaze when it turns opaque. 90% FZ-16 10% EPK 5% Copper Carbonate I have tried adding silica in incremental amounts of 1%, but this reduces thermal expansion and still yields me an opaque copper at that temperature. I was thinking Nepheline Syenite because of its high sodium content, but not sure if this is a misdirected effort. Next test will be a line blend of additional EPK at 1% increments to see if I can raise that firing temperature without reducing the crazing. Note, this is NOT for functional work.
-
If the total boron supplied is equal per pound of material, why do we perceive 3195 to be the superior boron source? In the context of weighing out recipes, 3134 and 3195 are the same, with many of the others (3124, 4131) being rather similar. Why not just base total ingredient contribution against the real world paradigm of weighing out ingredients by the pound/kg? I understand melting power is different because of other ingredients (and lack thereof), but speaking purely of boron, I’m getting the same amount scoop for equal scoop.
-
Thanks for the explanation @Bill Kielb and @Hulk. I will need to dive deeper into this, because it’s hard for me to wrap my head around the concept. Lucky I love this subject! I suppose my next question (and forgive my oversimplification of it) is: pound for pound of material, is the absolute boron amount I’m getting almost the same? I.e if I have a full scoop of 3195 and a full scoop of 3134, am I getting equal melting power from both? Or is the 3195 boron still double in that scoop?
-
It’s clear I don’t understand this well enough, because looking at the frit data sheets, I see those Boron levels to be the same. Is it that the total molecular weight is different between the two? I mean, why does the frit data sheet express these as a percentage in a comparison table, if they are not representative of the absolute values of each ingredient. Basically what I’m trying to do is have my glaze run more fluidly, so that spreads and fills the area between the ridges of my Cuenca style tile. At the moment, my glaze is melting just fine but if I apply it thickly, it will not melt and spread; it’s too stiff. I’m therefore positing that I need to “destiffen” the melt by removing alumina or increasing boron so that it melts much earlier. I’m aware this may be misguided however, and an alternative approach might be preferable.