Has anyone used Coyote cone 6 Crystal Glaze - particularly  Celadon or Lagoon ?  Are  they very runny and require a pedestal underneath the fired piece ? It calls for 2 brushed coats or 1 dipped coat- be intersted in hearing what others have experienced with these glazes. I was also wondering if  I extend my cool down  if the crystals might grow bigger.

 

heres is the firng schedule per Coyote :

100 deg/hr to 220 deg

350 deg/hr to 2000 deg

150/hr to 2200 hold for 15 min

500 /hr to 2150  hold for 15 min

125 /hr to 1400

 

 

 

 

below is the  firing schedule  i used for Laguna cone 5  Cyrstal Blossom Glazes

 

They are VERY RUNNY  and this schedule produced  smaller  crystals  just didnt like how runny the glaze was.

 

 

250deg/hr  to 1250

350deg/hr to 2140

25 deg/hr to 2165

1950  hold 3 hrs

 

 

anybody have any suggestions  with  the Coyote  glaze or  the Laguna glaze for that matter

Link to comment
Share on other sites

I have used them a few times yes. They like to be applied on the thinner side or they will run. A cookie or catch plate is a good idea just to be safe. They can be outstandingly beautiful but are difficult to work with. If dipping, a very quick in and out is needed or runs will be very bad. Hope this helps.

 

Jeri-Lynne

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.