mudpups

How to make stain into underglaze?

Recommended Posts

mudpups    0

I found a thread about this where someone gave a recipe - something like; 1 part stain, 1 part frit, 1 part bentonite. I kept the page open, went out to walk the dog, came back to get the recipe to make it and my computer had crashed - do you think i can find that thread again! NO!

 

Please, what was the recipe to turn a stain into an underglaze?

Share this post


Link to post
Share on other sites
Marcia Selsor    1,301

This is a recipe for low fire ^04 underglaze stain from Val Cushing.

By weight:

25 ep kaolin

25 frit 3110

25 stain....you can vary the stain for intensity. 25 or 1/3 is pretty intense.

 

This is mostly using for highlighting textured surfaces.

 

Marcia

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×