This ones for Cactus pots who asked about a yellow glaze this one works good in most applications -it can settle like a rock so use some Magama to keep it afloat.
cone 10 reduction ,Salt/soda,wood
Dolomite---- 23.63%
Nepheline Syenite- 71.55%
OM 4 Ball clay. 4.82%
For yellow salt
add: Zircopax. 17.92%
Red iron OX. 1.12%
Bentonite. 4.50%
For Blue salt
Add: Zirc
This ones for Cactus pots who asked about a yellow glaze this one works good in most applications -it can settle like a rock so use some Magama to keep it afloat.
cone 10 reduction ,Salt/soda,wood
Dolomite---- 23.63%
Nepheline Syenite- 71.55%
OM 4 Ball clay. 4.82%
For yellow salt
add: Zircopax. 17.92%
Red iron OX. 1.12%
Bentonite. 4.50%
For Blue salt
Add: Zirc