Not sure if this is what you're referring to, but there is a technique called "cementation glazing" that calls for placing small items such as beads in a container full of glazing powder. The powder nearest the items forms a glaze when it is fired. After firing, the glazed items break away easily from the remaining powder. This type of glazing is useful for items on which you don't want any firing marks or glaze-free areas (like beads) -- the glaze covers the item completely. This technique has been used for a long time in Iran; it is sometimes called the "Qom technique" after the city where it was observed in the 1960s. I've tried this a couple times with poor results -- I think I need to try it again. If this does interest you, I can provide some references with more information.

Link to comment
Share on other sites

Here are some references with information about cementation glazing:

 

Wulff, H. E., Wulff, H. S., & Koch, L. (1968). Egyptian faience: A possible survival in Iran. Archaeology, 21, 98-107.

 

Kiefer, C. & Allibert, A. (1971). Pharaonic blue ceramics: The process of self-glazing. Archaeology, 24, 107-117.

 

Tite, M. S., Manti, P., & Shortland, A. J. (2007). A technological study of ancient faience from Egypt. Journal of Archaeological Science, 34, 1568-1583.

 

La Delfa, S., Formisano, V., & Ciliberto, E. (2008). Laboratory production of Egyptian faiences and their characterization. Journal of Cultural Heritage, 9, Supplement 1, e113-e116.

 

And here is a web page with a photo of beads made with this method:

 

Donkey Beads—Iranian and Egyptian Faience

 

Hope this is helpful -- good luck with this!

Link to comment
Share on other sites

Just wanted to say that with the kind of glazing I'm talking about above -- cementation glazing -- the objects to be glazed are placed inside a container full of dry glazing powder. The glaze develops from an interaction between the object and the glazing powder during the firing. After the firing, the glazed objects break away from the remaining powder, which is friable and separates easily. This is one type of glazing of Egyptian faience (sometimes also called Egyptian paste) objects.

 

Deb -- I wonder if your student tried this cementation glazing method, or if you are maybe talking about the kind of Egyptian paste in which the glaze is created by ingredients in the paste of the object itself without any additional glaze materials (also known as efflorescence glazing). Could you tell us more about what your student did?

Link to comment
Share on other sites

  • 4 months later...

Here are some references with information about cementation glazing:

 

Wulff, H. E., Wulff, H. S., & Koch, L. (1968). Egyptian faience: A possible survival in Iran. Archaeology, 21, 98-107.

 

Kiefer, C. & Allibert, A. (1971). Pharaonic blue ceramics: The process of self-glazing. Archaeology, 24, 107-117.

 

Tite, M. S., Manti, P., & Shortland, A. J. (2007). A technological study of ancient faience from Egypt. Journal of Archaeological Science, 34, 1568-1583.

 

La Delfa, S., Formisano, V., & Ciliberto, E. (2008). Laboratory production of Egyptian faiences and their characterization. Journal of Cultural Heritage, 9, Supplement 1, e113-e116.

 

And here is a web page with a photo of beads made with this method:

 

Donkey Beads—Iranian and Egyptian Faience

 

Hope this is helpful -- good luck with this!

 

 

 

 

hi, i'm reza. i'm workin on this kind of glazzing. i wonder if u have any paper or ebook to mail me. i really feel disappointed with lack of trustworthy book or other kind of refrences and resources.

Link to comment
Share on other sites

Here are some references with information about cementation glazing:

 

Wulff, H. E., Wulff, H. S., & Koch, L. (1968). Egyptian faience: A possible survival in Iran. Archaeology, 21, 98-107.

 

Kiefer, C. & Allibert, A. (1971). Pharaonic blue ceramics: The process of self-glazing. Archaeology, 24, 107-117.

 

Tite, M. S., Manti, P., & Shortland, A. J. (2007). A technological study of ancient faience from Egypt. Journal of Archaeological Science, 34, 1568-1583.

 

La Delfa, S., Formisano, V., & Ciliberto, E. (2008). Laboratory production of Egyptian faiences and their characterization. Journal of Cultural Heritage, 9, Supplement 1, e113-e116.

 

And here is a web page with a photo of beads made with this method:

 

Donkey Beads—Iranian and Egyptian Faience

 

Hope this is helpful -- good luck with this!

 

 

 

 

hi, i'm reza. i'm workin on this kind of glazzing. i wonder if u have any paper or ebook to mail me. i really feel disappointed with lack of trustworthy book or other kind of refrences and resources.

 

p.s. my email add: reza.ala@gmail.com

Link to comment
Share on other sites

Egyptian paste is a self glazing body of high soda content. The flux migrates to the surface of the piece as it dries and fluxes into a glaze when fired.

I am wondering if this is what the original question was about.

Dry glazing, in my understanding, would be when the person is adding powdered glaze to a piece possible on top of a damp glaze that was already applied. I know of two friends who use this process to obtain interesting layered effects of glazing. Maybe Raza needs to clarify her original question. Egyptian faience is something quite different and very low temperature.

Marcia

Link to comment
Share on other sites

Hi Reza,

 

Since you quoted my response about cementation glazing, I'm guessing you might be interested in that. Cementation glazing involves placing small items (such as beads) in a container full of dry glazing powder. The glaze results from an interaction that occurs during firing between ingredients in the paste of the small item and ingredients in the dry glazing powder. This apparently ancient glazing technique was only (re)discovered and documented by researchers less than 50 years ago and there is not a lot of information available about it. The references I gave in my response above are the best, but they are not readily available in hard copy let alone online. Off the top of my head I can only think of one online document that might be helpful:

 

Faience Technology by Paul Nicholson (See pages 6-7 for a description of cementation glazing.)

 

Cementation glazing is one type of glazing of Egyptian faience (aka Egyptian paste). The other two are efflorescence glazing (the "self-glazing" that Marcia Selsor described that is most commonly associated with Egyptian faience) and application glazing (the painting on or dipping into a glaze slurry that many potters use today). Sometimes more than one glazing method was used on a single piece.

 

Let us know if this doesn't answer your question -- I'm happy to try again!

Link to comment
Share on other sites

I'm glad you liked the article, Marcia. Other than the beadmakers of Qom, Iran (here again is a photo of their donkey beads), the only person I know of who works with this technique is Jochen Brandt, and I don't really know a lot about his work. You can see some nice photos of a workshop he gave last year in Turkey here (hat tip to Ester Svensson). I would love to know about anyone else using this technique.

Link to comment
Share on other sites

I'm glad you liked the article, Marcia. Other than the beadmakers of Qom, Iran (here again is a photo of their donkey beads), the only person I know of who works with this technique is Jochen Brandt, and I don't really know a lot about his work. You can see some nice photos of a workshop he gave last year in Turkey here (hat tip to Ester Svensson). I would love to know about anyone else using this technique.

 

 

 

hi again, thanks for your help Amy.

maybe it's surprising for you. as i'd said before, i am working on this "donkey beads" (in farsi: khar-mohre) but i didn't tell u that i'm irainian, and i'm working in this issue excatly in "Qom". as u know, it considers as a traditional faience in iran so irainians take it for granted therefore i confront with a great lack of theorical resource for my univesity project . i've just rely on some people (great) experiences who have been working on it since long time ago.

(sorry for my poor english, i hope u can understand my words)

Link to comment
Share on other sites

Hi Reza,

 

I am very happy to hear that you are working on this! Hans Wulff is the person who observed and documented the cementation glazing process in Qom in the 1960s. (I should say he is the person who brought attention to this in the West -- maybe others have published information about this in Farsi or other non-Western languages? From what you've written it sounds like there are not many written resources about it.) Unfortunately, Wulff died shortly before the 1968 article I cited above was published. Here's an excerpt from a memorial article about Wulff:

 

 

Wulff, in fact, had just come up with the first satisfactory description of that process for yielding a glaze or faience termed "Egyptian blue." In a recently published article he tells how he and his daughter had finally gained the confidence of these craftsmen of the Iranian holy city of Qom who manufacture the famous "donkey beads" that tinkle about the byways of Iran. To the surprise of Wulff's ceramicist daughter, the technicians of Qom did not glaze the beads in any manner known to her but instead appear to use a variation of methods of salt glazing that involve both complex physical and chemical laws. With the help of Cyril Smith of the Massachusetts Institute of Technology and Leo Koch of the Department of Geology of the University of New South Wales, Wulff's researches were completed and have just been published. They provide a glittering example of what can still be accomplished by bringing a trained and inquisitive mind to bear on the secrets of ancient technology before all the traditional lore that connects us to that technology will have vanished from our earth.

 

(From Wertime, T. A. (1968). Hans Eberhard Wulff (1907-1967). Technology and Culture, 9, No. 3 (July, 1968), 459-461.)

 

 

One notable thing about this excerpt is the fact that the writer manages to use three terms to describe donkey beads in a single sentence (glaze, faience, and Egyptian blue). As you may have already discovered, a wide variety of terminology has been used to described this ceramic product. This can make it confusing when you are researching it. I think for the most part archaeologists and other related researchers have settled on the term "Egyptian faience" (even though it may not have been originally invented in Egypt) or "ancient faience" or even just "faience."

Your English is fine, by the way -- I am glad you found this forum and I hope we can be of help to you. Thank you for sharing the Farsi word for "donkey bead" -- I am glad to learn that. I would love to hear more about what you are doing, and I'm guessing others on this forum would, too. (I'm going to email you privately, too, to see if I can help with getting some more of this information to you.)

Link to comment
Share on other sites

Hi Reza,

 

I am very happy to hear that you are working on this! Hans Wulff is the person who observed and documented the cementation glazing process in Qom in the 1960s. (I should say he is the person who brought attention to this in the West -- maybe others have published information about this in Farsi or other non-Western languages? From what you've written it sounds like there are not many written resources about it.) Unfortunately, Wulff died shortly before the 1968 article I cited above was published. Here's an excerpt from a memorial article about Wulff:

 

 

Wulff, in fact, had just come up with the first satisfactory description of that process for yielding a glaze or faience termed "Egyptian blue." In a recently published article he tells how he and his daughter had finally gained the confidence of these craftsmen of the Iranian holy city of Qom who manufacture the famous "donkey beads" that tinkle about the byways of Iran. To the surprise of Wulff's ceramicist daughter, the technicians of Qom did not glaze the beads in any manner known to her but instead appear to use a variation of methods of salt glazing that involve both complex physical and chemical laws. With the help of Cyril Smith of the Massachusetts Institute of Technology and Leo Koch of the Department of Geology of the University of New South Wales, Wulff's researches were completed and have just been published. They provide a glittering example of what can still be accomplished by bringing a trained and inquisitive mind to bear on the secrets of ancient technology before all the traditional lore that connects us to that technology will have vanished from our earth.

 

(From Wertime, T. A. (1968). Hans Eberhard Wulff (1907-1967). Technology and Culture, 9, No. 3 (July, 1968), 459-461.)

 

 

One notable thing about this excerpt is the fact that the writer manages to use three terms to describe donkey beads in a single sentence (glaze, faience, and Egyptian blue). As you may have already discovered, a wide variety of terminology has been used to described this ceramic product. This can make it confusing when you are researching it. I think for the most part archaeologists and other related researchers have settled on the term "Egyptian faience" (even though it may not have been originally invented in Egypt) or "ancient faience" or even just "faience."

Your English is fine, by the way -- I am glad you found this forum and I hope we can be of help to you. Thank you for sharing the Farsi word for "donkey bead" -- I am glad to learn that. I would love to hear more about what you are doing, and I'm guessing others on this forum would, too. (I'm going to email you privately, too, to see if I can help with getting some more of this information to you.)

 

 

 

hi amy,

 

thanks for your helpful information.

I think I should mention that I'm studying Material Science (Ceramic Engineering). there is just a few articles in Iran which are written from the engineering point of view. Most of them are written by the students who studied on traditional handicraft so they have artistic perspective that is not very useful for my thesis.

Link to comment
Share on other sites

Hi Reza,

 

It is interesting to know that you are coming at this from a materials science point of view. You may already know this, but one author to look for is Pamela Vandiver. She has done a lot of research on Egyptian faience from a materials science point of view. In case it might help someone else researching Egyptian faience, here are two books in particular to look for (as far as I know, neither of these books is available in digital format):

 

Ceramic masterpieces: art, structure, and technology (this is a great book on the production technology of all kinds of ceramics; though it is not specific to cementation glazing, it includes one chapter on the manufacture of an Egyptian faience chalice)

 

and

Ancient Egyptian faience: an analytical survey of Egyptian faience from predynastic to Roman times (although it is nearly 30 years old, Vandiver wrote an appendix on Egyptian faience technology that is very thorough and is still cited)

 

 

Good luck with your work on this, Reza -- if you are able to share some of your findings with us, I hope you will.

Link to comment
Share on other sites

Hi Reza,

 

It is interesting to know that you are coming at this from a materials science point of view. You may already know this, but one author to look for is Pamela Vandiver. She has done a lot of research on Egyptian faience from a materials science point of view. In case it might help someone else researching Egyptian faience, here are two books in particular to look for (as far as I know, neither of these books is available in digital format):

 

Ceramic masterpieces: art, structure, and technology (this is a great book on the production technology of all kinds of ceramics; though it is not specific to cementation glazing, it includes one chapter on the manufacture of an Egyptian faience chalice)

 

and

Ancient Egyptian faience: an analytical survey of Egyptian faience from predynastic to Roman times (although it is nearly 30 years old, Vandiver wrote an appendix on Egyptian faience technology that is very thorough and is still cited)

 

 

Good luck with your work on this, Reza -- if you are able to share some of your findings with us, I hope you will.

 

 

 

Hi amy,

thanks, again lots of good info.

be sure that I will do.

Link to comment
Share on other sites

  • 1 year later...

Wanted to update this thread with a link to a facebook page that shows the work of modern day Egyptian faience (Iranian faience) potters:

خرمهره kharmohreh. Blue beads. Iranian Faience

 

This post shows fired beads still embedded in the cementation glazing powder:

 

fired beads in cementation glazing powder

 

This page appears to be public and available for all to view, so you shouldn't need a facebook account to view it. Lots of photos of beads and more with that brilliant blue glaze.

Link to comment
Share on other sites

  • 6 years later...
On 5/15/2013 at 11:13 PM, Amy Waller said:

This post shows fired beads still embedded in the cementation glazing powder

 

On 7/8/2011 at 3:05 PM, Reza said:

I think I should mention that I'm studying Material Science (Ceramic Engineering). there is just a few articles in Iran which are written from the engineering point of view. Most of them are written by the students who studied on traditional handicraft so they have artistic perspective that is not very useful for my thesis

Hi

Thanks for the literature . All there is on the subject.

I see the conversation is from 2015...I will try nevertheless:

On the video the men are first embedding the beads in  a huge amount of something, that sure isn't glaze, and then they fire them.

If Reeza could post her research... would be nice

 

 

 

 

Link to comment
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

 Share

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.