i am looking for a simple (student makable) true gloss white...

 

thanks, ruth

 

Ruth, I haven't tested this glaze but I remembered reading about it that is was a simple glaze to make. It's Tony Hansen 5X20 plus 10% zircopax White Gloss here's the formula 20-Frit 3134 20-EPK 20-Silica 20-Custer Spar 20-Wollanstonite 10-Zircopax. I read a review of a test by Alisa in Denmark, she said that Cobalt, RIO, Black Stain. Chrome and Yellow Ochre showed well under the glaze held their edge and stayed exactly as painted. Test away!

Link to post
Share on other sites

i am looking for a simple (student makable) true gloss white...

 

thanks, ruth

 

 

Ruth, I haven't tested this glaze but I remembered reading about it that is was a simple glaze to make. It's Tony Hansen 5X20 plus 10% zircopax White Gloss here's the formula 20-Frit 3134 20-EPK 20-Silica 20-Custer Spar 20-Wollanstonite 10-Zircopax. I read a review of a test by Alisa in Denmark, she said that Cobalt, RIO, Black Stain. Chrome and Yellow Ochre showed well under the glaze held their edge and stayed exactly as painted. Test away!

 

 

a thousand thanks! i'll let you know how it tests out.

Link to post
Share on other sites
  • 3 weeks later...

i am looking for a simple (student makable) true gloss white...

 

thanks, ruth

 

 

Ruth, I haven't tested this glaze but I remembered reading about it that is was a simple glaze to make. It's Tony Hansen 5X20 plus 10% zircopax White Gloss here's the formula 20-Frit 3134 20-EPK 20-Silica 20-Custer Spar 20-Wollanstonite 10-Zircopax. I read a review of a test by Alisa in Denmark, she said that Cobalt, RIO, Black Stain. Chrome and Yellow Ochre showed well under the glaze held their edge and stayed exactly as painted. Test away!

 

 

i tested this... pretty nice glaze, a bit of streaking. for the most part, useful (especially for students.) thanks again!

Link to post
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.