Can anyone tell me why my tiles that were previously fired to ^5 would break during a ^05 firing? I added an overglaze and refired to a much lower temperature. So why would they break at this point? Very frustrating!! Is there a trick as to how to fire this last firing? Ie. different than a bisque firing? Peeps in...peeps out...slow fire/cool? I fired preprogrammed at standard rate. Should I change this? Thanks for your help. Linda

Share this post


Link to post
Share on other sites

Many forms, especially flat ones, do not like to be refired. They don't handle the thermal shock and uneven heating very well. The top of the tile heats faster than the bottom of the tile and they crack. Try firing on stilts of some sort- even little clay coils or wads would work, or slow down the firing at the beginning and end.

Share this post


Link to post
Share on other sites

thanks, neil, i wondered the same thing.  thought it might have to do with placement on the particular shelf in the same spot in the kiln.  shelves change shape without warping so we notice it .  have been taking pictures of the loading so i can refire in the same location if needed.

Share this post


Link to post
Share on other sites

Thanks Nell. Makes sense. But, will I not have problems with warping if they're on stilts?

In my experience, no.

The clay itself should not be moving much at those low temps ... I don't think your over glaze would cause warping.

But I could be wrong as my work is mainly with porcelain.

Share this post


Link to post
Share on other sites

 

Thanks Nell. Makes sense. But, will I not have problems with warping if they're on stilts?

In my experience, no.

The clay itself should not be moving much at those low temps ... I don't think your over glaze would cause warping.

But I could be wrong as my work is mainly with porcelain.

 

 

I'm thinking the same as Chris. A cone 6 clay should not have warping issues at low fire temps. But as always, test it first, and make sure the tile is evenly supported.

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.