I have used a few bags a year of alberta slip  (still have a few bags of albany left) over many years now

I have found that its about the same in some applications and not the same in others. It as Wyndam says may need flux as true abany fluxes at a cooler temps I think. In my black glaze which only has three ingredients (which I posted here last year Nep sye and cobalt ox and alberta) its a direct albany pound for pound deal

In other glazes more flux may be needed especially at cone 6. Albany alone melts very well at cone 8-9

I have not run tests on Alberta alone lately-maybe years ago but I have no recall of the results.

Mark

Share this post


Link to post
Share on other sites

 

Any favorite ( or marginally like able). Albany/alberta based glaze recipes?

 

 

In Daniel Rhodes book there is a section on slip glazes.

With some of the info above, one of these glaze people may be able to formulate it for you, or work around with the Frit suggested.

Rhodes

Cone 9-10

Albany SLip      60

Cornwall stone  25

Iron oxide            5

Whiting              10

Beautiful  dark iron red. in Reduct.

THIckly applied Tends green black

 

 

and

 

 

Albany slip   65

Neph Syn    35

Khaki in Ox, Iron red in Red.

Hope this helps

Babs

Share this post


Link to post
Share on other sites

I use this one at cone 6 all the time. I use it with no colorant layered with 2 or 3 other glazes but I have used the brown in the past.

 

ALBERTA SLIP     80%

NEPH SY   10%

G.B.   10%

Add

RIO 4% for Brown

Add

RIO  4%

Coblat Carb. 3% for black

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.