Ok having only used commercial glaze, I would love to try mixing one on my own. Does anyone have a recipe for a pretty light peach / melon color? Cone 5-6 As simple as possible?

 

 

Alas, you have run into a range of color that is a little more difficult without the use of a stain. Most orange and red colors as your melon is between the two are more difficult at ^6. So I would start with a base opaque, and add a Mason stain. Others might have a recipe that depends on the interaction of chromium and tin, but I don't have one for that color.

Share this post


Link to post
Share on other sites

This recipe is a ripe cantaloupe color.

 

EPK14.00g Silica26.00g Wollastonite14.50g F-4 Feldspar24.00g Frit 324920.00g

 

Add 5% of Mason stain 6121

 

Good Luck!

Darrel

Share this post


Link to post
Share on other sites

Darrel

 

I can't wait to try your ripe cantaloupe glaze but a little confused with the Frit. Is that 20 grams of Frit 3249? My eye sight isn't great and I can't quite make it out.

Sorry if that's a dumb question.

 

Thanks

 

Gary Taylor

Share this post


Link to post
Share on other sites

Gary, looks like 20 grams is what Darrel was saying. Looks like an interesting glaze. if you like the look of the finish, which looks like it should be a gloss, you could use this as a base glaze and use other stains to get a wider pallet of glaze colors.

Wyndham

Share this post


Link to post
Share on other sites

Darrel

 

I can't wait to try your ripe cantaloupe glaze but a little confused with the Frit. Is that 20 grams of Frit 3249? My eye sight isn't great and I can't quite make it out.

Sorry if that's a dumb question.

 

Thanks

 

Gary Taylor

 

 

Yes, 20 grams of frit 3249

Share this post


Link to post
Share on other sites

The clear base glaze that Darrel posted, G1215U, is a wonderful clear for low expansion clays. It's expansion is 5.71 so it's probably going to shiver on a lot of clays. Min

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.