hi all, i'm having some problems with slip casting, as you can see after 25 minutes my pieces are very defectives, i cannot figure out with this issue. the slip respect water ratio given (it is pc010b porcelain, should be 4,1 liter per kg porcelain) and works well in small one piece mold (espresso cup dimension). the photos shows a water glass 2 pieces mold.

thank you for your time

giorgio

IMG20230918111553 (1).jpg

IMG20230918111852.jpg

Link to comment
Share on other sites

2 hours ago, giorgiodidon said:

hi all, i'm having some problems with slip casting, as you can see after 25 minutes my pieces are very defectives, i cannot figure out with this issue. the slip respect water ratio given (it is pc010b porcelain, should be 4,1 liter per kg porcelain) and works well in small one piece mold (espresso cup dimension). the photos shows a water glass 2 pieces mold.

Can you confirm your slip recipe.

Potterycrafts gives 18.5 litre of water to 50 Kg powdered clay (i.e. 0.37 litre water to 1 Kg powdered clay).
https://www.potterycrafts.co.uk/Products/pottery-powdered-clays/P3103

Walkers give 9 to 12 litres water to 25 Kg powdered clay (i.e. 0.36 to 0.48 litres of water to 1 Kg powdered clay)
https://shop.walkerceramics.com.au/AW500.B/Limoges-PC010B(CM10)-Porcelain-~25kg/pd.php

Can you confirm that you didn't use freshly-made casting slip, as it takes a while to fully hydrate the clay (e.g. overnight).

Edited by PeterH
Link to comment
Share on other sites

I'd hoped that one of the experts would have commented by now.

Looking your pictures.

inSidePot_small.jpg.668b55ee37d2ed3c2f7306fd3c350b12.jpginside2_small.jpg.5296339399f7b2353f2420ea34b8f462.jpg

Is the one on the left a casting of the water glass, and the one on the  right a casting of the espresso cup?
Do you have any idea why the two surfaces look so different.
Did you do anything differently when making the casts or the moulds.

 

Looking at the first picture. The inside is very uneven and I've no idea why, so I'll just mention a few possibilities ...

Defective slip?
- Was the slip nice and uniformly smooth: as it went into the mould and as it came out. No lumps or uneven  "thickness" or jelling.

Defective mould?
- Did you buy it or make it yourself.

Defective plaster?
- What plaster did you use, and what was the ratio of plaster to water

Contaminated surface?
- Did you use a parting agent when you cast the mould.

Damp mould?
- How did you dry the mould after making it. How long did you dry it for.

Outside OK?
- Can you confirm that the outside of the casting is smooth and uniform.

PS I wouldn't change your slip until you have some idea why the two castings came out so very differently.

Link to comment
Share on other sites

@giorgiodidon, did you check the weight of the slips against the chart that is available for those slips? From one of the links that Peter linked: https://shop.walkerceramics.com.au/documents/sr/WC-AW500-SR.pdf

Do you have a Ford cup (or something equivalent to those) to measure viscosity / fluidity?

Did you add any additional deflocculants? I've never mixed a slip where the deflocculants are included in the mix, @Jeff Longtin, could this be the issue? I'm seeing a greenish film inside the lumpy casting, floc issue? 

Link to comment
Share on other sites

Hi all, both photos same thing, I have tried with 2 water porcelain ratio first 0.41 liter per kg and also 0.39 liter per kg, settled for 2 days and sieved. I think at this point that the problem is in mold, It is an Italian plaster I used 1 to 1 water plaster ratio, and used soap for demolding. I noticed that bumps in the pieces are the same in every piece, so  it must be a mold issue. I made a mold 70 water 100 plaster but it is too thick, pouring very difficult, I'll try with some more water (waiting mold dry)

Giorgio

Link to comment
Share on other sites

4 hours ago, PeterH said:

https://www.potterycrafts.co.uk/Products/pottery-powdered-clays/P3103
Deflocculants are added in the spray drying of this clay so it is not necessary to add them.

Yup, I read that too, the other link has a link to the one I posted above (slip recipe) and has Dispex at 1 - 12.5 grams per 25kg of dry mix.

For sure the plaster needs to be mixed at the correct water:plaster ratio. 

Link to comment
Share on other sites

A couple things:

plaster - if mixing 70-100 results in a thick mixture, and you only mix for 2-3  minutes, its likely you have old plaster. Adding more water helps with the pour but it will result in soft plaster. (Also takes longer to set up.) New plaster would be a good start.

slip - If you don't know if, or what, deflocculant was added to the clay before you purchased it, it may be best to first attempt to make a slip with a decent flow. Add enough water to get a decent flow and let the mix sit overnight. See how much it thickens overnight. In the morning add some more water if it needs it. 

Its been my experience that if the slip is over deflocculated it will gel up in the mold no matter how thin you mix it. 

If the slip has too much water you will mostly get an extremely thin casting. I've never gotten a lumpy pour with too much water. Lumpiness is mostly a case of deflocculation issues.

Mold soap - did you allow the soap to dry before pouring the plaster? If it was still wet it could seal the surface of the plaster and slow the absorption of water.

Laguna Clay sells their B-mix in a powder form in a "Casting" version. They list the recipe on their website. What their website does not indicate is that the "Casting" version also contains the dry form deflocculants, soda ash and barium, already mixed into the dry powder. 

Link to comment
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.