Can you put two pieces that have fallen off with a combination of paper clay and Magic Water? I had a braid fall off of one of my student pieces. I slipped and scored and applied a paste of toilet paper, slip from the same clay body and magic water??

 

I packed the crack and the site around the braid. If this doesn't take I am guessing the alternatives are: 1) wait until the piece fires and simply glaze and using epoxy reattach; 2) use some silica (which I don't have) and gently put these back together before firing; and 3) place the braid right next to the joint and apply glaze liberally and hope and pray.

 

What is magic water? I know it is supposed to be good stuff so I bought it when I got my clay supplies but haven't used it yet. Will it be a good adherent? Am I on the right track in terms of mending this piece?

 

Do know that the piece is wrapped now and I am trying to dry it slowly again with the crack filler.

 

Nelly

Link to post
Share on other sites

That is a good site. I have used paper clay to repair both green and bisque ware.

I use a toilet paper and clay body recipe with vinegar, karo syrup and a little water.

For bisque repair I wet the bisqued area very well and then add the paper clay. It works.

Marcia

Link to post
Share on other sites

Sometimes you can mix some table salt or Epson salt into your slip, and use this to join parts. The salt can help flux the clay parts and help in sticking. Keep in mind though that salt is a flux in the kiln too and you need to wipe away any excess.

Link to post
Share on other sites

Sometimes you can mix some table salt or Epson salt into your slip, and use this to join parts. The salt can help flux the clay parts and help in sticking. Keep in mind though that salt is a flux in the kiln too and you need to wipe away any excess.

 

 

Dear Yedrow,

 

When you say "flux" what exactly do you mean?? I have heard that salt in an electric kiln can produce noxious gases and cause damage to the kiln wiring. When you say flux do you mean that it may melt??

 

Thank you all for your responses.

 

Nelly

Link to post
Share on other sites

That is a good site. I have used paper cal to repair both green and bisque ware.

I use a toilet paper and clay body recipe with vinegar, karo syrup and a little water.

For bisque repair I wet the bisqued area very well and then add the paper clay. It works.

Marcia

 

 

Marcia, I like your ingredients for making a paper clay mud! May I ask for proportions & instructions on using the vinegar, karo, and water?

Thanks, Jayne

Link to post
Share on other sites

That is a good site. I have used paper cal to repair both green and bisque ware.

I use a toilet paper and clay body recipe with vinegar, karo syrup and a little water.

For bisque repair I wet the bisqued area very well and then add the paper clay. It works.

Marcia

 

 

Marcia, I like your ingredients for making a paper clay mud! May I ask for proportions & instructions on using the vinegar, karo, and water?

Thanks, Jayne

 

 

Dear Marcia,

 

I have never heard of using Karo syrup before. I am guessing Karo is the same as corn syrup. So far so good. My piece is holding and I have been building layers up slowly. Will see what happens. Thank you for the vinegar and karo suggestions. It is helpful to have this information.

 

Nelly

Link to post
Share on other sites

I use paper clay slip for just about all my joins, and paper clay and slip for repairs. My formula is slip from whatever clay I am using, a drop or two of dish detergent, to help with the mold, and a dash of sodium silicate, or other suitable defloculant (not too much). Add an amount (30-40% volume of slip) of paper that has been shredded and soaked in boiling water until the water cools. Drain the paper, reserving the liquid to make more slip, mix it all together, using a blender or juicer, and it is ready to go.

 

I attach all kinds of things with this stuff. Bisque to bisque, green to green, green to bisque, and repair glazed pieces and refire. You don't need to worry about it drying too fast, it will be just fine. I have used it to adhere different types of clay. No problem seems to be too bad for paper clay.

 

For big cracks, I dry some of my slip mixture on a plaster bat and use it to roll coils. For easy application of the slip in hard-to-reach places, use a cake decorating bag filled with the not-too-wet slip, and pipe it into the cracks.

 

I love paper clay for repairs. I may one day get around to actually making something with all paper clay.tongue.gif

Link to post
Share on other sites

I use paper clay slip for just about all my joins, and paper clay and slip for repairs. My formula is slip from whatever clay I am using, a drop or two of dish detergent, to help with the mold, and a dash of sodium silicate, or other suitable defloculant (not too much). Add an amount (30-40% volume of slip) of paper that has been shredded and soaked in boiling water until the water cools. Drain the paper, reserving the liquid to make more slip, mix it all together, using a blender or juicer, and it is ready to go.

 

I attach all kinds of things with this stuff. Bisque to bisque, green to green, green to bisque, and repair glazed pieces and refire. You don't need to worry about it drying too fast, it will be just fine. I have used it to adhere different types of clay. No problem seems to be too bad for paper clay.

 

For big cracks, I dry some of my slip mixture on a plaster bat and use it to roll coils. For easy application of the slip in hard-to-reach places, use a cake decorating bag filled with the not-too-wet slip, and pipe it into the cracks.

 

I love paper clay for repairs. I may one day get around to actually making something with all paper clay.tongue.gif

 

 

 

Dear All,

 

I have a jug of slip that I use for joining. I have also used vinegar straight- up on the seams I don't want to split open. I add this after I slip and score. I must say, I pay attention to detail and slow drying so having something split or break off is a bit new to me.

 

I am the type that wraps my handles individually with 2 inch strips of plastic to ensure adhesion I am that preoccupied with drying times and no cracks.

 

Nelly

Link to post
Share on other sites

I have had good results with Amacos bisque fix

Mark

 

 

Dear Mark,

 

I did look this stuff up. I think it means that you take two bisque pieces and put them back together again with this compound. I will watch for it when I am in the pottery store next. Looks good.

 

Thank you,

 

Nelly

Link to post
Share on other sites

I've read that you can mend cracks in bisque by mixing 90% ground bisque, 5% glaze, and 5% gum. I've yet to try it though.

 

 

Sounds interesting and makes sense. I have made a mixture of silica and I think it was glaze and put two pieces together once. It worked but I must say, it bothered me having to do something to save the piece. I like my pieces to go into the kiln and come out the way I put um in. I pride myself on no breakage and running of glazes. But I guess when you are trying to give small classes, this is part of it. I will let the group know how my pieces turn out. I have fired overnight and the kiln should be ready to crack this afternoon. I will know if the braid held or not with the paper clay and magic water. If not, we go to all of these wonderful suggestions and I figure something out. Will keep you posted.

 

Nelly

Link to post
Share on other sites

Dear All,

 

I have just unloaded the kiln. The braid did stay attached with the layers of paper clay and magic water. All looks well except a crack developed where I never expected it to on this piece. Perhaps, like someone said on this forum, the crack was there when it went into the kiln and I just didn't see it?? All and all, I am quite pleased at the result. I will, however, be cautious in handling this piece until after it is 100% glazed and fired for good. ;) Thank you for all the great advice one and all. Even the thin pieces as directed (i.e., bed of sand and tile) turned out well. Great advice. Nelly

Link to post
Share on other sites

Nelly

We fire a 35 cubic foot car kiln once a week with a bisque then a glaze (cone 10) we see cracks- knock stuff off and toss in the trash pottery on a regular basis. We have leaned after 39 years what works and what does not and what may work. We as you strife for perfect pots but at the volume I produce things can go sideways and there is some loss rate. I never bisque twice any pot ever for me its a time space waste.

I repair pots with Aztex High Fire mender(you mix this with your clay body really works well)bisque fix and sp-mender by Amaco and claymaker XL Plus refractory cement.

We fill cracks or toss the pot-attach thumb spots on handles or other items. After a while you learn what can and cannot be done in ceramics in terms of repair. Pie plate rim cracks are a toss it out deal.

If we fix it we glaze and fire it same day-if its in green state we fix and bisque it.

As far as runs we all strife for zero but my bench grinder and two dremel tools get a work out at times. Thats just part of ceramics.

Here is todays bisque at 9 am and glaze loaded about 6 pm-this is what happens almost every friday here-fire Saturday unload Monday-

The one thing in ceramics is you cannot count on it till its done.

Mark

Link to post
Share on other sites

Dear Mark,

 

Yup, that is a LOT of pots. I guess I do expect some cracking and I am pretty fastidious about what is waste worthy and what isn't. I do, now, have a shard pile. It is my own pile and not that of a studio of potters so it is clear what I waste and don't. Like you, I have got to know how far I can push certain clay forms and what will work or will fire. Given that this was my first time working with students, I was filled with angst. They all want their piece to turn out well and as the teacher, you too want these same things for them. All and all, I think I am happy. The one crack is in a place between the eyes. Rather than fix it or try to patch it, I think I will suggest she utilize it in her design. You know something like using it for its artistic merit in making facial glasses on her piece. The broken nose that I repaired with a different colored clay, I will suggest gently that she could do something like maybe a harlequin design. All and all though, I am happy. Thanks for the good words of advice regarding knowing when to keep and things and when to throw the towel in so to speak. It is important to realize this and after all, as I say to myself, "it is just mud." Thanks for the pics! Nelly

Link to post
Share on other sites

Just repair it and glaze. Let it dry in between, and let it dry well after glazing, before firing.

 

 

 

Does anyone use Magic Mender?

 

 

I’ve used Magic Mender for fixing hairline cracks with perfect results. I’ve also successfully used Magic Mender to fix slightly wider hairline cracks by adding ground up bits of bisque ware to the Magic Mender.

 

 

Link to post
Share on other sites

That is a good site. I have used paper cal to repair both green and bisque ware.

I use a toilet paper and clay body recipe with vinegar, karo syrup and a little water.

For bisque repair I wet the bisqued area very well and then add the paper clay. It works.

Marcia

 

Here is where I got the original spooze recipe. I have added paper pulp, about 20% of the dry clay in quantity.

Peggy Herr was an early clay art participant. She developed this recipe. She died in 2006.I add paper pulp to this.about 20% to the clay portion.

This is her recipe.

1/3 parts dry clay powdered....any body...preferably the one you are using

with no grog

1/3 parts heavy karo syrup

1/3 parts white distilled vinegar

 

A drop of hydrogen peroxide to keep it from spoiling...it will bubble for a

few minutes and then settle down. if you dont add that the sugar goes bad

and smells awful in about a day.

 

 

Link to post
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.