Hi, 

I’m firing earthenware at 1050 C using a commercial Ferro glaze. 

I can’t seem to find a fix for this nasty drip marks when dipping.. In this particular case the specific gravity was 1.5, too high, recommended is 1.4. but even at 1.4 i’m getting drip marks.

My guess is the glaze is under flocculated, can someone correct me if i’m wrong? epsom salts probably don’t help, tried on a small batch, i guess theres little to no clay.

i’ve made it thixotropix by adding an additive similar to OPTAPIX G1308 (binder and flow agent). that made it a little better but not good enough.

I’d love to hear your thoughts on how to go about this issue.

 

https://imgur.com/gallery/odrmHGD

Link to comment
Share on other sites

Those nasty drip marks look like a slip texture on the cup...but if they are that persistent, I'd look for a different glaze to work with. I'm not a dipper, so I've never experienced this before. Have you fired any of the pieces yet? If not, give it a shot and see what you come out with. You might like the effect. If you have, what does it look like?

Link to comment
Share on other sites

Tony Hansen's suggestions https://digitalfire.com/4sight/library/thixotropy_and_how_to_gel_a_ceramic_glaze_73.html have been very helpful for me.

I use Epsom salts (or vinegar).

Have found that a good grip is also helpful, for it allows me to give the piece a downward shake and twist+flip to fling away gathering drips; from there I'll run any remaining drip around and around the rim ...once the glaze is set up, I'll wet a finger and smooth the drip (if any). Timing is important; practice helps. Be sure to stir before each application - that thin layer of more watery glaze at the surface will wreak havoc.

Good luck!

Edited by Hulk
two goods
Link to comment
Share on other sites

The specific gravity won’t affect how the glaze drips but the rheology, or how the glaze flows will. This is the thixotropy of a glaze, or lack thereof. While I am a fan of Tony Hanson, Sue Macleod is a much more thorough and effective teacher on this subject. Her explanations are far more approachable. She goes into more depth on how to troubleshoot and fix things. 
https://suemcleodceramics.com

Epsom salts would have been my first choice to fix a dripping issue. How much did you add, and was it thoroughly incorporated? Did you add your Epsom salts as dry material, or did you add them as a small amount of a super saturated solution?

Link to comment
Share on other sites

First, do the drips show after firing? With many glazes it's a non-issue, especially if you're layering and letting it run anyway. It looks to me like the glaze is simply too thick. Thin it out a little, then increase the dip time to compensate. In my studio, I mix the glaze so they're like a creamy chocolate milk consistency, then dip for 6 seconds. My glazes are a bit more watery than a lot of other studios that my students have worked in, but it gives them more control over the thickness of the application.

Link to comment
Share on other sites

For forms like those in the linked image I would pour the inside then hold the pot by the foot ring and dip the outside. Hold it upside down and slowly rotate the pot. Let any surplus glaze roll around the rim edge to avoid a drip when you turn it right side up. Touch up any spots where your fingers held the pot with a brush.

Link to comment
Share on other sites

2 hours ago, Callie Beller Diesel said:

The specific gravity won’t affect how the glaze drips but the rheology, or how the glaze flows will. This is the thixotropy of a glaze, or lack thereof. While I am a fan of Tony Hanson, Sue Macleod is a much more thorough and effective teacher on this subject. Her explanations are far more approachable. She goes into more depth on how to troubleshoot and fix things. 
https://suemcleodceramics.com

Epsom salts would have been my first choice to fix a dripping issue. How much did you add, and was it thoroughly incorporated? Did you add your Epsom salts as dry material, or did you add them as a small amount of a super saturated solution?

I made a super saturated solution and kept adding to a small batch. I didn’t notice a difference, i was looking for thixotropy, mainly how it swirls backwards after you mix it. 

epsom salts from my understanding change the charge of the clay particles in the glaze, i assume this glaze has little to no clay. Wasn’t able to find a full composition of this glaze on Ferro’s website.

Link to comment
Share on other sites

1 hour ago, neilestrick said:

First, do the drips show after firing? With many glazes it's a non-issue, especially if you're layering and letting it run anyway. It looks to me like the glaze is simply too thick. Thin it out a little, then increase the dip time to compensate. In my studio, I mix the glaze so they're like a creamy chocolate milk consistency, then dip for 6 seconds. My glazes are a bit more watery than a lot of other studios that my students have worked in, but it gives them more control over the thickness of the application.

So i thinned it out to 1.4 SG, much thinner now, similar composition like you’re describing. I’ve increased the additive by 0.15%, i can feel it’s more thixotropic now, meaning that it bounces back more when you mix it.

I’ll have to check tomorrow to see how much it settled, i assume it won’t settle too much.

Here’s the test dips, 5 second dip.

Not perfect.. the final result will look good for this matte clear glaze.

eventually i want to add some color, smallest unevenness will show as a darker color and looks bad in my opinion. Trying to get the most even drip :)

DehrmWU.jpg

1rO1me7.jpg

 

Link to comment
Share on other sites

2 hours ago, Callie Beller Diesel said:

The specific gravity won’t affect how the glaze drips but the rheology, or how the glaze flows will. This is the thixotropy of a glaze, or lack thereof. While I am a fan of Tony Hanson, Sue Macleod is a much more thorough and effective teacher on this subject. Her explanations are far more approachable. She goes into more depth on how to troubleshoot and fix things. 
https://suemcleodceramics.com

Epsom salts would have been my first choice to fix a dripping issue. How much did you add, and was it thoroughly incorporated? Did you add your Epsom salts as dry material, or did you add them as a small amount of a super saturated solution?

thixotropy is the issue indeed.. increased it a little and that extends the drying time and allows it to flow more.

for really large pieces the flow time was too little, and quickly built up in some areas.

Link to comment
Share on other sites

@Mitzuuu89 I used to use a lot of true celadons years ago, and learning about thixotropy was a game changer for sure. With Epsom salt solution or any other additive, you have to add just a little at a time and mix for a minute or two before it becomes noticeable. If you overshoot it goes horribly wrong. 

Link to comment
Share on other sites

11 hours ago, Mitzuuu89 said:

, i assume this glaze has little to no clay. Wasn’t able to find a full composition of this glaze on Ferro’s website.

FYI- The general goal is 10% to let’s say 20% clay to help with maintaining suspension.

Edited by Bill Kielb
Link to comment
Share on other sites

  • 9 months later...

Hello,

I recently purchased two mugs from an extremely well established pottery house in the UK.  My issue was that they both came with a single slip drip mark running down the inside of each mug! I didn't consider this deliberate or right at all, rather a nasty fault.  Little wonder they were the last two left, as I later discovered! Any thoughts on this please?

 

Many thanks

 

Link to comment
Share on other sites

6 hours ago, Neleh said:

Any thoughts on this please?

I wouldn’t sell them to you if they were mine. When I make high quality mugs I try to ensure there are no defects including diamond polishing the foot so it has little chance of scratching what you set it on. Just my idea of what a quality mug from me ought to be though. I don’t sell things with drips unless they are decorative. Of course we spray many of our glazes just to cover things evenly. It’s not likely the drip will hurt the functionality if it’s just minor though.

Edited by Bill Kielb
Link to comment
Share on other sites

There is a segment of the population that does value such maker’s marks, and that don’t consider them to be flaws. I don’t mind the odd drip and will leave some in on purpose, as long as they fit the aesthetic I’m going for. That said, leaving them on purpose is different than having them there by accident. If you’re concerned, it might be worth it to bring it up to the pottery you bought them at.  Not knowing which pottery it is, it’s hard to say if it was deliberate on their part or if the two mugs just snuck past QC. 

Link to comment
Share on other sites

Proper craft/technique requires the same arduous learning and application of said knowledge as needed to produce any other expert production that meets  basic + known standards. Clay work/ceramics is no different-----there's a right way, a wrong way, and a just plain too lazy to learn how to do it right way.  Selling functional ware with flaws (however minor) is hugely different from intentionally deviating from the best practices, based on the rigors of chemistry/science/kiln operations etc. and centuries of ceramic knowledge. Allowing such "flaws" to live is a specific philosophical approach and (in my world) may be considered a benign opposition to the ethos of perfection, or a statement about ignoring the elephant in the room, depending on the context of the piece. I just started a wall mask, which from the git-go breaks a bunch of correct craft technique applications/rules and will ignore many others before it is done.  I'll stick a pic in Studio Operations/Making Work.

Link to comment
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

 Share

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.