VladCruceanu

Photo lithography on clay - nothing transferred

Recommended Posts

I have used the following tools:

- Roller

- Arabic Gum Liquid

- Indian Ink

- Tried two pictures: 1. Printed in color by a laser Xerox. 2. Copied black and white by another Xerox machine.

Made everything as in the video: https://www.youtube.com/watch?v=jUNH6KvYGnk

Tried 2 times with both pictures on soft leather hard clay and nothing transferred.

Please help me understand what I am doing wrong. 

 

 

Arabic Gum Liquid.png

Indian Drawing Ink.png

Roller.png

Share this post


Link to post
Share on other sites

Lithography is based on the fact that oil and water don't mix. The gum-arabic solution
provides the water-based part, so you need to use an oil-based ink.

A printable description of the process can be found at https://pistrucciartworks.wordpress.com/2011/03/20/photolithography-on-clay/

Regards, Peter

Hope you have more success than I did. Lithography works better with high-contrast images, and sometimes
fudges such as half-toning are required.

Edited by PeterH
Repeatedly edited to overcome finger-trouble!

Share this post


Link to post
Share on other sites

I would suggest starting with DIY ink --  oil+pigment (a mason stain sounds good[1]). [2]
.. and an image with some largish 100% back and 100% white areas.

Everybody seems to say no to inkjet printers. Some [all?] Xerox and Laser printers produce
a fused plastic image that is likely to be good at rejecting water and being receptive to oil.
While inkjet inks may be water-soluble.

After you've applied the gum-arabic solution and let things stand for a while you should
see that the paper in the white areas has absorbed the solution (e.g. looks translucent).
It needs to do this to repel the oil.

Regards, Peter

[1] Use an oxide until you've got the hang of things, if you don't have any to stain hand

[2] Ideally it should be what's known as a drying oil. Several are listed in https://en.wikipedia.org/wiki/Drying_oil.
These can be bought (fairly expensively) as artists supplies. Oils sold for cooking  are cheaper. However as long shelf-
life and optimum drying properties  are mutually exclusive  the cooking oil may be denatured [to prevent it going
rancid too fast after opening]. Personally I would start with something like walnut oil from the local supermarket.
... remember drying properties are pretty academic until you get the transfer process working.

For  production use an artists/woodworkers/decorators linseed oil might be technically better. Up to you to judge
the cost/performance balance. But be aware that  rags soaked in the more drying oils can [and sometimes do]  burst
into flames, and have been the cause of some expensive fires (linseed and tung oil in particular).  [AFAIK keep rags in
a small screw-top jar. If things start to go downhill the oxygen is depleted before  the temperature rises too high.]

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.