I think I have two in an my old clay mixing book-Its been 35 years since I have used these-not sure on thin strength .These are all cone 8-10

All old school stuff here

 

Mark

casting porcelian

spar 25

epk 40

flint 25

ball clay 10

+sodium silicate 1/4 of 1% or 1/2 tsp

strain 6-8 times-60-80 mesh screen

 

Pats casting porc slip

EPK 2.5 lbs

ball clay 2.5 lbs

silica 2.5lbs

spar 2.5 lbs

 

HSU casting porc slip

3 gal.

EPK 25 3405

Ball clay #4 25 3405

Feldspar 25 3405

Silica 25 3405

Sodium Silicate 34

Soda Ash 34

12 lbs.

Add deflocculants to water 1st

4 lbs H20 for 10 lbs. clay

 

when I had a slip casting business for 12 years we used darvon instead of sodium silicate to deflocculate it works better-we cast 40,000+ candle lamps

and gave up on soda ash as it hard on the plaster molds over time

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.