Looking for a good Robin's egg blue glaze - cone 6 oxidation.

I've thought about taking an existing commercial glaze - Mid South Turquoise and perhaps adding a little copper carbonate and/or cobalt carbonate.

I know it would be an experiment but it's not quite turquoise enough for me.

Any thoughts?

Share this post


Link to post
Share on other sites

Another way is to add Mason stain to a good ^6 clear . . .

 

So Clear ^6

Frit 3124 32.2%

Soda Feldspar -- Kona F4 (Minspar) 25.8%

Silica 19.4%

Whiting 12.9%

Kaolin -- EPK 9.6%

 

Add 5% Mason Stain #6464 for Robin's Eggshell Blue

 

(recipe from Michael Sherrill workshop)

 

 

Share this post


Link to post
Share on other sites

I love this robin's egg blue! It is buttery matte/satin and opaque.

 

Nepheline Syenite 60

ball clay OM4 8

lithium carb 1

strontium carb 22

flint 9

 

add

copper carb 1.5

titanium dioxide 3

 

 

Thanks! This sounds wonderful...I'm always looking for different blues....

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.