I have a recipe that is from a Walter Ostrom workshop. The glaze is called ^04 Moon. The ingredients don't add up to 100, and I'm wondering if I should go ahead and test it as written. Just thought I would see if anyone had any comments or suggestions.

Thanks, Pam

Mag carb 25

EPK 10

Lithium carb 5

Borax 20

Gerstley borate 10

Share this post


Link to post
Share on other sites

If you rebalance the 70 to 100 parts, then it is a glaze from Linda Arbuckle's handouts called Moon, firing Cone 06-04, less the copper carbonate that made the Arbuckle handout glaze turquoise. See below:

 

Glaze name: Moon

 

Cone: 06-04

 

Color: Turquoise

Testing:

Surface: Crater

Firing: Oxidation

Glaze type: Texture

Transparency: Opaque

Recipe:

Magnesium carbonate 35.70

Kaolin 14.30

Lithium carbonate 7.10

Borax 28.60

Gerstley borate 14.30

Copper carbonate 7.10

Comments: Bob Shay sculpture glaze.

 

I suppose the Magnesium carbonate is what makes the surface "crater" and the glaze type "texture". Sounds like fun!

 

John

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.