So, Ive been playing with a few 'lava' style glaze recipes to obtain a similar effect to this:

 

 

KkiKBYa.jpg

 

Using silicon carbide yields some wonderful bubbling and crawling but the color is pretty much dark grey or darker at cone 5/6.

 

Lava recipes..:

 

slip   100

silicon carbide 10

 

calc. carbonate (whiting)       25

feldspar                        50

epk                             12.5

silica  (quartz)                12.5

 

silicon carbide                 12.5

 

Now something I read, is barium sulfate can be a substitute for silicon carbide here.  Which sounds great to me because its cheaper and lighter colored, and I want to get as close to white as possible with the glaze.  However, nothing I do with barium sulfite in the above recipes has the same effect, all I end up with are these weird peeling crawls that look very little like lava and very much like scar tissue.  Interesting maybe but not really the direction I wanna go.

 

So Im wondering if anyone here has actually use barium sulfate specifically for a good lava glaze effect?  Thanks!

 

Link to post
Share on other sites
  • 2 weeks later...

 

KkiKBYa.jpg

Using silicon carbide yields some wonderful bubbling and crawling but the color is pretty much dark grey or darker at cone 5/6.

 

 

 

I've recently started playing with SC, my first test only used 3.4% SC and fired to ^6 it was white. (There's also a  bit of green glaze showing at the top). Using more SC has just given me a nasty black result.   I would try reducing the amount of SC.

 

post-7271-0-69240100-1467321047_thumb.jpg

post-7271-0-69240100-1467321047_thumb.jpg

Link to post
Share on other sites
  • 2 weeks later...

 

 

KkiKBYa.jpg

Using silicon carbide yields some wonderful bubbling and crawling but the color is pretty much dark grey or darker at cone 5/6.

 

 

 

I've recently started playing with SC, my first test only used 3.4% SC and fired to ^6 it was white. (There's also a  bit of green glaze showing at the top). Using more SC has just given me a nasty black result.   I would try reducing the amount of SC.

 

attachicon.giflava.jpg

 

 

 

you know what?  that's gorgeous, and i'm taking your advice into the shop tonight.  thank you.

 

im well into that dark black vibe and i got some really interesting textures but couldnt get that lovely color you got, which i reallllly wanted.

 

4fxgLp8.jpg

 

D0shwoj.jpg

Link to post
Share on other sites

No, but I have used it to create this unusual effect.

 

 

It was spot brushed on after the glaze had dried. It created the matte/gloss offset. 0.50% as I recall. Dang-giving away secrets.

Nerd

Wow Glazenerd.

It looks like out of focus background. Really interesting crystals.

Marcia

Link to post
Share on other sites
  • 3 years later...

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.