This is a glaze posted on 12/4 /10 in response to a request for a yellow buttercup , not mustard glaze

Marci’s Matt ^6 Reduction

 

EPKaolin 1150 23

 

Dolomite 1000 25

 

Neph Syenite 1900 38

 

Silica 900 18

 

Whiting 200 4

 

Gerstley Borate 500 10

 

Variables:

 

Blue 1% Cobalt Carb

 

LightGreen1.5%Nickel Carb + 1.5%RedIron Oxide

 

Gray 2.5% Rutile +1.5% Nickel Carb

 

Warm Blue 1% 1% Cobalt Carb+ 5% Manganse Di

 

Tan 6% Manganese Di. +2.5 Red Iron Ox +1%

 

Rutile OR try using only 5% Rutile as a colorant

 

 

 

 

This particular example has 4% vanadium stain, 4% Rutile and 3% zircopax. To brighten it up , reduce the zircopax

From the album:

forum discussions

  • 7 images
  • 0 comments
  • 11 image comments

Photo Information for yellow glaze

 Share


Recommended Comments

Do not use Vanadium on surfaces with contact with food. It is toxic. This glaze is very easy to manipulate color. For a food safe buttery yellow , eliminate the vanadium increase the rutile, reduce the zircopax to a lower %

 

 

Marcia

Link to comment

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Add a comment...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.