dhPotter 472 Posted November 13, 2020 (edited) Report Share The customer wanted a very plain plate. Customer also wanted a tan with little to no rust breaking. It took well over 100 test tiles to develop. Then numerous plate firings to get the glaze application thickness just right. This glaze was developed by mixing a clear at 60% and a matte at 40%. The color was developed by adding 2% rutile, 2% tin oxide and 1.6% RIO. The glaze has some visual movement. This glaze is food safe with no cutlery marking. Cutlery dragged across the glaze has little to no sound. The glaze does not physically move when fired - stays where you put it. Edited November 15, 2020 by dhPotter glazenerd and Hulk 2 Quote Link to comment