I've been off the forum for a while. Paying job has been in the way since April. Finally getting back in the studio. Hooray! I'm looking for recipes for both gloss and matte warm (chocolate) brown glazes at ^ 5-6. I usualy use Buncomb White clay, but playing with Mary's Porcelian and Hellious. Suggestions and pics welcome! Thanks! P

Link to comment
Share on other sites

New Tyler Amber, Cone 6 Oxidation

(amber/root beer glossy glaze)

 

Red Art, 60

Frit 3110, 20

Gerstley Borate, 20

Total, 100

 

John's10X (John Britt)

(satin black (you can sub a brown Mason Stain instead of black), Cone 6 Oxidation)

 

Soda feldspar, 10

Spodumene, 10

Silica, 10

Wollastonite, 10

Kaolin, 10

Ball Clay, 10

Dolomite, 10

Talc, 10

Frit 3134, 10

Frit 3195, 10

Base Subtotal, 100

 

for black, Mason Stain Black 6600, 5

Bentonite, 2

Total, 107

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.