Biglou13 Posted July 31, 2014 Report Share Posted July 31, 2014 Ok "celadon-ish" I made some Nice color. It crazes, it's known to craze. Anyone up the silica? Any improvmentS? Link to comment Share on other sites More sharing options...
Marcia Selsor Posted July 31, 2014 Report Share Posted July 31, 2014 what is the formula?Does it craze on all clay bodies? How is it cooling? What type of firing? Marcia Link to comment Share on other sites More sharing options...
Biglou13 Posted July 31, 2014 Author Report Share Posted July 31, 2014 "burke's strong celadon-ish". 58 feldspar. 17 whitting. 14 flint. 6 om4. 5 zinc oxide, 1 copper carb. (+- copper for degree of green) Controlled cool. I look for schedule Link to comment Share on other sites More sharing options...
Marcia Selsor Posted July 31, 2014 Report Share Posted July 31, 2014 How fast did it cool? Sometimes crazing comes from cooling too fast. What clay was it on? Have you tried it on more than one clay? Marcia. Link to comment Share on other sites More sharing options...
Tyler Miller Posted July 31, 2014 Report Share Posted July 31, 2014 I'll bet it's crazing because of all the feldspar. Feldspar's got a pretty high COE due to the potash and soda. This is why the original celadons craze. Reformulate so that you get what's supplied by the feldspar from other sources and cut the soda/potash and sub in another flux. The whiting could use some adjustment, too--that's the highest COE in the recipe. Insight is your friend here. Frits too. Link to comment Share on other sites More sharing options...
Marcia Selsor Posted July 31, 2014 Report Share Posted July 31, 2014 Biglou, I think Ty has something. Although Glenn Nelson's base for ^6 has 64% Custer Feldspar, no silica 18 whiting , 9 ball clay 5 talc. That is it. Here are some celedons I used in Reduction and one for ^6 Oxidation They all have much more silica Celedon^6 Reduction Whiting 18.5 Neph. Syn 25.8 EPKaolin 18.8 Silica 31.1 Gerstley Borate 4.6 Red Iron Oxide 1.5 AACC Celedon Cone 6 Color: light to medium green Tested Surface texture: glossy Type of firing: Reduction Glaze type: Ca Ingredients: Percent Batch Flint 31.00 1550 Nepheline Syenite 30.00 1500 Gerstley Borate 21.00 1050 EPK Kaolin 10.00 500 Whiting 8.00 400 Totals 100.00 % 5000 gm Also add: Iron Oxide 1.00 50 Comments: May use up to 3% Iron oxide to intensify color Possible Health Hazards: Flint: free silica-wear a NIOSH approved dust mask when handling dry material This is one for Oxidation Selsor Faux Celedon ^6 OxidationWhiting 18.5Neph Syen 25.8EPK 18.8Silica 31.1Gerstley B 4.698.8Copper carb 0.3Mason #6600 Black 0.02 Link to comment Share on other sites More sharing options...
Tyler Miller Posted July 31, 2014 Report Share Posted July 31, 2014 I'd say the presence of boron in all the glazes except Glenn Nelson's is significant. Nelson's seems to have a pretty high COE, even still. Where I'd want my COE if I were to have a deliberate craze. Link to comment Share on other sites More sharing options...
Min Posted July 31, 2014 Report Share Posted July 31, 2014 There is silica in the Nelson celedon, it's coming from the custer. Silica level is a bit low in the Burke celedon but the expansion is so high you would need to add a lot of silica to fix it and the end result would be a glaze doesn't look like the original. It's the sodium and potassium that are the problems, coe's are high because of them. Burke celedon is a gloss isn't it? Do you have a clear that fits your clay without crazing? I would start by working on finding a clear base that pools then add copper and or stains to get the colour you are after. I've got a lot of good clear recipes, let me know what kind of clay you are putting it on if you want a few to try with different coe's. This is a good thing to do with several clear glazes then run the tests through accelerated crazing tests to know the glaze coe that fits your clay for this and future glaze work. There are other factors that come into play but this gets you in the ballpark. Link to comment Share on other sites More sharing options...
Marcia Selsor Posted August 1, 2014 Report Share Posted August 1, 2014 Min, There is 64% feldspar in Nelson's and 58 % feldspar ( we don't know what feldspar) in Burkes. I know there is Silica in feldspars. but crazing is from several things, not fitting the clay, COE incapatible with clay body or cooling too fast, over firing, or too thick of an application. I agree he needs to add more silica even though there is a lot of flux as supplied by the feldspar, whiting and zinc.I supplied the recipes as a none technical way to look at the recipes and make a comparison. burke's is short on silica. Link to comment Share on other sites More sharing options...
Wyndham Posted August 1, 2014 Report Share Posted August 1, 2014 I recently did a test on strong celedon and got crazing as well. I will try Marcia's to see how that goes. I was wondering if adding some zircopax, about3 % might help and get a cloudy celedon. I've seen zircopax change copper(1%) from a yellow green to a blue(er) green in several different test. Just another path to explore Wyndham Link to comment Share on other sites More sharing options...
Min Posted August 1, 2014 Report Share Posted August 1, 2014 I recently did a test on strong celedon and got crazing as well. I will try Marcia's to see how that goes. I was wondering if adding some zircopax, about3 % might help and get a cloudy celedon. I've seen zircopax change copper(1%) from a yellow green to a blue(er) green in several different test. Just another path to explore Wyndham Have you tried Leah Lietson's chun? It is similar looking to Burkes even though it's not a celedon, has that translucent pooling quality without being overly glossy. It crazed on the clay I was using at the time but with a slight increase in silica it worked. It has some similarities to Burkes. Alumina is a bit low so it might need a bit of tinkering there to bring it up a bit if used on food surfaces. . Base works well with stains also.(photo is of Leitson's work) of My version: Whiting 14 Zinc 12 Minspar 38 OM4 6 Silica 34.5 (original has 30) Bentonite 2 Copper carb 0 point 3 up to 2 point 0 ^6 oxidation Link to comment Share on other sites More sharing options...
Wyndham Posted August 2, 2014 Report Share Posted August 2, 2014 thanks, that's a beauty I'll have to try. Wyndham Link to comment Share on other sites More sharing options...
jrgpots Posted August 2, 2014 Report Share Posted August 2, 2014 Biglou, I think Ty has something. Although Glenn Nelson's base for ^6 has 64% Custer Feldspar, no silica 18 whiting , 9 ball clay 5 talc. That is it. Here are some celedons I used in Reduction and one for ^6 Oxidation They all have much more silica Celedon^6 Reduction Whiting 18.5 Neph. Syn 25.8 EPKaolin 18.8 Silica 31.1 Gerstley Borate 4.6 Red Iron Oxide 1.5 AACC Celedon Cone 6 Color: light to medium green Tested Surface texture: glossy Type of firing: Reduction Glaze type: Ca Ingredients: Percent Batch Flint 31.00 1550 Nepheline Syenite 30.00 1500 Gerstley Borate 21.00 1050 EPK Kaolin 10.00 500 Whiting 8.00 400 Totals 100.00 % 5000 gm Also add: Iron Oxide 1.00 50 Comments: May use up to 3% Iron oxide to intensify color Possible Health Hazards: Flint: free silica-wear a NIOSH approved dust mask when handling dry material This is one for Oxidation Selsor Faux Celedon ^6 Oxidation[/size]Whiting 18.5[/size]Neph Syen 25.8[/size]EPK 18.8[/size]Silica 31.1[/size]Gerstley B 4.6[/size]98.8[/size]Copper carb 0.3[/size]Mason #6600 Black 0.02[/size] Marcia what would these celadons be like if I were to add crimson mason stain? I'm looking for a red transparent "celadon" glaze. Would these glazes work for this? Jed Link to comment Share on other sites More sharing options...
drmyrtle Posted August 3, 2014 Report Share Posted August 3, 2014 Min Marcia, Have you tried this recipe from digital fire? G1216M Cone 6 Ultraclear for porcelains Material Amount Units +/- *Stat Minspar 200 8.60 kg Frit 3134 23.20 kg Wollastonite 15.20 kg EPK 24.80 kg Talc 4.30 kg Silica 23.80 kg 99.90 Has anyone else had experience with this? Link to comment Share on other sites More sharing options...
Marcia Selsor Posted August 3, 2014 Report Share Posted August 3, 2014 Min Marcia, Have you tried this recipe from digital fire? G1216M Cone 6 Ultraclear for porcelains Material Amount Units +/- *Stat Minspar 200 8.60 kg Frit 3134 23.20 kg Wollastonite 15.20 kg EPK 24.80 kg Talc 4.30 kg Silica 23.80 kg 99.90 Has anyone else had experience with this? I have used 1214 but found it to be too shiny for my needs. There are many good glazes on there. Marcia Link to comment Share on other sites More sharing options...
Min Posted August 3, 2014 Report Share Posted August 3, 2014 Min Marcia, Have you tried this recipe from digital fire? G1216M Cone 6 Ultraclear for porcelains Material Amount Units +/- *Stat Minspar 200 8.60 kg Frit 3134 23.20 kg Wollastonite 15.20 kg EPK 24.80 kg Talc 4.30 kg Silica 23.80 kg 99.90 Has anyone else had experience with this? Yes, I have tried that recipe. It is a very nice clear on most surfaces although there is a problem with it. Tony Hanson and I had a long back and forth email discussion about it. We both found it formed rough microcrystaline patches, (his term), especially where it broke on ridges and rims. Tried firing cooler, glazing thicker, no soak, long soaks etc, couldn't solve it. He went on to come up with the MK3330 clear that uses strontium frit Fusion F 524 to address the problem with G1216M, however when I tried it it crazed horribly. I can no longer find it on his site but if you want the recipe let me know. The clear I'm currently using is a 50:50 blend of G1216M and G1215U, fits my ^6 "porcelain" without crazing and has none of the microcrystaline patches. No milky boron clouding on the white clay I use or over the underglazes, needs to go on fairly thick. Link to comment Share on other sites More sharing options...
drmyrtle Posted August 5, 2014 Report Share Posted August 5, 2014 Thank you for sharing. Link to comment Share on other sites More sharing options...