Jump to content

Nuka Ash Crackle Cone 6 Glaze


jrgpots

Recommended Posts

Here is my first successful ash glaze.  I call it Nuka crackle.  it is fired to  ^6 oxidation.  It is placed on thick and cracks as it dries. The top of the tile is double dipped while the bottom is single dipped. It does not drip, but has a great matte finish.

 

The recipe is:

 

Soda Feldspar                40

Tumbleweed ash             26.7

Whiting                            13.3

EPK                                 13.3

Frit 3124                            6.7

 

Total                               100

 

I'm thinking of using it over a darker glaze so the color is seen through the cracks.

 

Jedpost-26461-0-99677600-1402437293_thumb.jpg

post-26461-0-99677600-1402437293_thumb.jpg

Link to comment
Share on other sites

This is great! What clay body? Is this like real tumbleweed ash that you make?

Look forward to seein more test!

The test tiles are from Reclaimed clay, a mix of laguna cone 6 clays...lots of moroccan sand, eletric brown, and half half.

 

Yes, it is real tumbleweed ash. My back yard collects them by the thousands.

 

Jed

Link to comment
Share on other sites

What kind of glaze would you use to maintain that crawl?

 I made a glaze with  a local bentonite clay.  The base glaze is a nice transparent camel color. But then  I added 10% rio. I  layered theash glaze  on top.  The ash glaze absorbed some of the rio and turned a bit yellow.  But it did not run and the base glaze was visible between the cracks. I'm hoping to get a better base glaze that brings out the ash glaze more.

 

recipe:

 

local bentonite             76

Neph sys                     18

gersley borate               6

 

Total                          100

 

add 10% RIO.

 

 

Jed

post-26461-0-49077000-1402457344_thumb.jpg

Link to comment
Share on other sites

I would bet if you increased the frit to about 10% (off the wall guess) it might bead up more, which might also look interesting.

I like the tumbleweed idea. Tumbleweed might have a higher silica ratio than other ash sources and be a bit stiffer.

Just a thought.

Wyndham

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information