I am looking for a good stable clear liner glaze that does not have a tendency to craze. I found this in a past post with a reply from John Britt but its for cone 6

Mastering Cone 6 Glazes
GLOSSY CLEAR LINER cone 6
20.00 G-200 Potash Feldspar
20.00 Ferro 3134
15.00 Wollastonite
20.00 EPK China Clay
6.00 Talc
19.00 Silica

Does anyone know its range. If I take it to cone 7 - 8 will it still be stable? I am really searching for a good stable non crazing clear liner type glaze for this temperature.

#2 neilestrick

neilestrick

    Neil Estrick

  • Members
  • PipPipPip
  • 4,192 posts
  • LocationGrayslake, IL

Posted 22 April 2014 - 09:04 AM

Try it at 7. It may be fine. If not, you could always stiffen it up a little bit by adding more EPK. Any recipe you find will have to be tested for crazing, because it all depends on which clay body you are using.


Neil Estrick
Kiln Repair Tech
L&L Kilns Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

[email protected]


#3 cambriapottery

cambriapottery

    Advanced Member

  • Members
  • PipPipPip
  • 39 posts
  • LocationCanada

Posted 22 April 2014 - 05:41 PM

Thanks for the input Neil. I will try it for sure.





Also tagged with one or more of these keywords: clear glaze, liner glaze, cone 7, stable glaze

0 user(s) are reading this topic

0 members, 0 guests, 0 anonymous users