I have done bullnose years back, by rolling out a slab the same as the tiles I am using, then carving a credit card to the shape I wanted and scraping the new tiles until rounded. Do it when cheese to almost leather hard. We have also done edging tiles with an extruder die as Ben says.

Link to comment
Share on other sites

OK you just mean a round over-like this edge on my tile in photo.

I had a friend who made custom tile in the 80's and he had all the stuff-table cutter -tile extruders-whatever-I just used his stuff with my clay and took it home and dried it and glazed it-I threw the sink and I used to sell custom ones as well . No more of that stuff.

Just use the card like Pres said to cut it down then just sponge it smooth-these tiles are all near 4x4 inch cone 10 stoneware.

The glaze is a old time fav that I used for 20 years but gave up as I'm not working with stoneware anymore except for salt ware.

I think it came from Alfred and I altered it in glaze calc class in school. 

The original is Tin Ox-8 with no zircopax- my recipe is below

I changed it to lower cost to school when I was the glaze tec in 1974

This also requires a reduction atmosphere to look great.

This job on one of our bathrooms is sanded grout and done with a wet diamond saw. The sink round  tiles where made custom round for the sink in two sets-Made to fit this layout from wet greenware.I still have a fired spare set in case I break one.Always best to

plan ahead.

 

Wamo Mamo II

 

potash spar-(custar)-49

China Clay (EPK)-----21

Whiting----------------4

Dolomite--------------19

Tin Oxide--------------4

Zircopax---------------4

Total -----------------101

 

Application thickness is KEY-thin it breaks brown thick its white-looks best on an Iron spot body like these tiles of mine.

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.