I'm having an issue with one of my glazes cracking as it dries on the bisque. The problem is worse when it is put over another glaze. This of course leads to crawling on the fired ware. I've tried using Veegum T to toughen it up, but not to much effect. I have just inherited some CMC, but I don't know how to use it. Is that a possible solution to this problem? Or do I need to do something else?

 

Joel.

Share this post


Link to post
Share on other sites

I'll try the bentonite. From what I've read though, bentonite can cause the same problem. I was trying to avoid this effect. Would a 1-2% mix avoid exacerbating the problem?

Marcia, It is pretty thin and I still have the problem. At the moment the glaze has a specific gravity of 1.47. I need a solution that will keep this sg. If I'm understanding the articles I've read about CMC, it can toughen the glaze. But, I don't know how to use it. From what I've read there is a learning curve to this material.

 

Joel.

Share this post


Link to post
Share on other sites

I'm not a big gum user but have used it in salt kiln coatings for adhesion.

heres the ceramic arts daily stick-

 

Carboxymethylcellulose (CMC) — an organic gum used as a suspension/adhesion agent in glazes. Normally, a small amount of gum is added to a quart or so of warm water and left overnight. Once dissolved, this solution may be added in small doses to glazes, slips, and engobes to improve application performance. Source: Clay: A Studio Handbook

 

 

Share this post


Link to post
Share on other sites

That usually happens to me with commercial glazes that get too dry in the jars. i have tried remixing with water, using the additive Amaco sells and nothing seems to revive them. Now i just throw them out if i see them cracking on the bisque.I hate to throw money into the trash can. Anyone have any luck with this?

Share this post


Link to post
Share on other sites

This is the recipe. There isn't a lot of EPK in it so I don't think that is the problem.

 

Custer Feldspar............. 24.1
Gerstley Borate............. 13.8
Wollastonite................ 5.8
Magnesium Carbonate......... 2.5
Barium Carbonate............08.6
FRIT 3134................... 8.7
FRIT 3195................... 2.3
EPK Kaolin.................. 9.9
Silica...................... 24.2
Rutile...................... 8.0
red iron oxide.............. 1.0

 

I'm working on a newer version of this glaze so the problem could fix itself. I'll do a test on it this week.

 

Custer Feldspar............. 25.17
Gerstley Borate............. 17.70
Magnesium Carbonate......... 2.61
Barium Carbonate............ 4.29
FRIT 3134................... 9.09
EPK Kaolin.................. 10.34
Silica...................... 30.80
Rutile...................... 8.00
red iron oxide.............. 1.00 

Share this post


Link to post
Share on other sites

I have two commercial  cone 6 glazes that have laid around and settled/dried up some. I've mixed them up, but they crack after being applied to bisque. They seem to have adequate water. Can anything be done to correct this?

Share this post


Link to post
Share on other sites

....The problem is worse when it is put over another glaze....

We have few glazes that are "clay based" and they do not like frit based glazes when applied to bisque ware... or was it the other way around.

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.