 I am spraying a couple of layers of egg shell glaze on some test tiles.  the first layer is slightly less than 1 mm thick and it is sticking fine. the second 1 mm layer, applied some days later, is sometimes peeling away from the first layer of glaze.

 

however, on the majority of tiles,, it works just fine. I can't figure out what the difference is between the handful of tiles that  the second layer peals away from the first when dried and those that it sticks just fine.

Share this post


Link to post
Share on other sites
Mark C.    1,807

When I have glaze issues like this and I do . I suggest not letting your 1st glaze get so dry and spraying when it still is not bone dry.

I have this issue with freehand brush work-The sooner I can get that second glaze on the less issues of it coming off.

Another idea is-

You could mist a very little 1st and see if this helps it stick better?

Mark

Share this post


Link to post
Share on other sites
Pres    896

That is also what I have found from double dipping. Don't let the first layer get too  dry or when the second goes on the first gathers the water and top peels away.

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×