I've got a request for some mugs that have a matt yellow on the outside bottom 2/3. I have Mamo that I use as a matt but what OI need is a more yellow matt to satin and I'm wondering about Alfred yellow or Ferguson yellow. Does anyone have any experience with a good gas fired c10 r yellow.

 

Several recipes I've seen call for 15% zircopax and 3.7 % iron ox. I just don't know what that would look like.

Thanks Wyndham

Link to comment
Share on other sites

  • 3 weeks later...

Duney is a nice yellow ^9/10 reduction glaze

Neph Syenite   71.5

Dolomite          23.5

Ball                    5

 

add

Zircopax             7-9

Bentonnite         2.5

Red Iron Ox.       1.3

 

I know it looks like a weird recipe and I remember it does run when thick, but is beautiful.

r

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.