What is the best way to colour porcelain black? My thoughts were just to try adding some black iron oxide to the slip.

 

Looking to make slip cast moulds for cups and saucers to be black on the outside and white on the inside.

Share this post


Link to post
Share on other sites

What is the best way to colour porcelain black? My thoughts were just to try adding some black iron oxide to the slip.

 

Looking to make slip cast moulds for cups and saucers to be black on the outside and white on the inside.

 

 

 

Reply by Stuart Altmann: Iron oxides can produce a surprising range of colors, depending just on firing temperature and kiln atmosphere during firing alone. That is because iron has five(?) oxides, each with its own color. For example, a common, simple iron glaze recipe from Penland--I'm on the road now and don't have the formula memorized--starts with Fe2O3 (common 'red rust' ) and gives either a dark tomato red or jet black. In cone 10-11 in electric oxidation firing, this gives a dark tomato red, with various amounts of irregular black splotches.

Share this post


Link to post
Share on other sites
bigDave    4

What is the best way to colour porcelain black? .

 

 

Maganese Dioxide and iron ox, are cheaper and can give nice dark tones, but fluuuxxxx the clay so what ever you are currently using...

 

Test

 

I use 6% Mang-ox in buff ^5 slip, and drop 4 cones to accomodate the lower melt/flux , make a nice dark dark brown

 

 

That is a starting place perhaps

post-12771-136943158919_thumb.jpg

post-12771-136943158919_thumb.jpg

Share this post


Link to post
Share on other sites
Marcia Selsor    1,301

Manganese Dioxide is toxic ,penetrates the skin, fumes are bad as is ingestion.

I wouldn't use it in a clay body. If I use it in a glaze I don't have my hands in it. Dave Shaner thinks it is what effected his health. Hans Coper also. Cheap is not necessarily wise.

Marcia

Share this post


Link to post
Share on other sites
Chris Campbell    1,087

I thought Chris would jump in here. This is her area of expertise

. I would recommend using Black mason Stain #6600.

But check the blogs on Chris's website.

http://ccpottery.com

 

Marcia

 

You are right Marcia ... It's called 'best black' too ... It is very black at about 8%.

Share this post


Link to post
Share on other sites
bigDave    4

 

 

You are right Marcia ... It's called 'best black' too ... It is very black at about 8%.

 

Thats precious ...@ 94.55 usd for 5 pounds...

 

Id be right out of business.

 

Thanks for the concern ladies, good motives

 

And good luck testing, High Bridge Potter

 

 

Big D

Share this post


Link to post
Share on other sites

Well after some testing here is the black that I have produced. Porcelain (unknown recipe) 2 parts to 1 part black iron oxide.

 

I found that the natural clay was a much deeper black than when I added a transparent glaze on top. I think that is partially because the transparent has a slight white tinge to it.

 

Anyway turns out it is near perfect for a saucer unglazed which is a bonus :D and my saucer glazing technique is a little rough at best. All turned out quite nice as I didn't want to try other colorants. I just trust iron oxide, maybe I am uninformed but it seems safe to me.

 

297528_167013483476214_1863917124_n.png

 

Share this post


Link to post
Share on other sites
OffCenter    82

Well after some testing here is the black that I have produced. Porcelain (unknown recipe) 2 parts to 1 part black iron oxide.

 

I found that the natural clay was a much deeper black than when I added a transparent glaze on top. I think that is partially because the transparent has a slight white tinge to it.

 

Anyway turns out it is near perfect for a saucer unglazed which is a bonus biggrin.gif and my saucer glazing technique is a little rough at best. All turned out quite nice as I didn't want to try other colorants. I just trust iron oxide, maybe I am uninformed but it seems safe to me.

 

297528_167013483476214_1863917124_n.png

 

 

 

Usually the pictures inserted into posts are too big but this one is too small. That is a really interesting cup and saucer but the picture is too small for me to get a good look at it. Do you have other cup & saucers?

 

Jim

Share this post


Link to post
Share on other sites

Yes it is a little small, I will sort out a bigger one sometime this week. My co-worker who is a good photographer was not in the studio. I had to battle with his complicated camera which is why it ended up so little. I can sort out a better resolution sometime this week smile.gif

 

I could not get the camera to focus on the work unless I was 2 meters away, never been able to understand lenses, apertures and so on...

 

I should have designed and fired the 'final' idea soon so will post some more then and grab a few pictures of other tests.

Share this post


Link to post
Share on other sites

Manganese Dioxide is toxic ,penetrates the skin, fumes are bad as is ingestion.

I wouldn't use it in a clay body. If I use it in a glaze I don't have my hands in it. Dave Shaner thinks it is what effected his health. Hans Coper also. Cheap is not necessarily wise.

Marcia

 

 

Marcia,

I think you are incorrect with regards to manganese penetrating skin, it has been explained to me that because of the particle size of MnO2 and the fact that it is not soluble it cannot be absorbed through skin. I do know that it can cause mild skin irritation in some people, perhaps this is what you were thinking?

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×