Posted 23 May 2013 - 08:00 AM

I run a women's project in Namibia ( Africa) We have had so much trouble with our clear glazes over underglaze that I am switching to Majolica style using Stoke and coat. It's so expensive to ship from the USA, so I thought maybe I could at least make the base glaze myself, although I am a complete newbe to glaze making ! We primarily make beads, so a brush on glaze is preferred, but we could adapt if necessary. Oh and the preferred temp. for stoke and coat is cone 06........it can go higher, but any dimensional is lost . Thanks for any help
Val

#2 Iforgot

Iforgot

    Advanced Member

  • Members
  • PipPipPip
  • 155 posts
  • LocationColorado

Posted 23 May 2013 - 08:18 AM

I have a recipe that is for firing at cone 04, stroke n' coats will lose none of their color at ^04. This recipe can be brushed to dipped, try to keep the application thin though.




Linda Arbuckle Majolica:

frit 3124 65.8

F-4 feldspar 17.2

EPK 10.8

neph sy 6.2

100.0

+ tin 4

+ zircopax 9

+ bentonite 2


Derek VonDrehle

Raku, Pit fired, Majolica, and Stoneware ceramic artisit

#3 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 6,361 posts
  • LocationRed Lodge, Montana

Posted 23 May 2013 - 10:56 AM

spray with a stay flo laundry starch to harden the glaze surface before painting overglazes.
Linda has detailed handouts online.

Marcia
Marcia Selsor, Professor Emerita,Montana State University-Billings
[http://www.marciaselsorstudio.com

#4 TJR

TJR

    Advanced Member

  • Members
  • PipPipPip
  • 1,821 posts
  • LocationWinnipeg,Manitoba,Canada

Posted 23 May 2013 - 12:55 PM

Marcia,Iforgot;
Why have you /she got two soda spars in the recipe? Could you go with 23.4 of one or the other? I have Neph Sy, I do not have Kona F-4, but I could probably get it.
TJR.
I have not used this glaze, but was thinking about mixing up a batch.
T.

#5 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 6,361 posts
  • LocationRed Lodge, Montana

Posted 23 May 2013 - 03:24 PM

If you can run it through a computer system to work it into one soda spare, go ahead. I just think it is simple the way it is. Iy mixes up nice and creamy. I figure don't mess with a good thing.

Marcia
Marcia Selsor, Professor Emerita,Montana State University-Billings
[http://www.marciaselsorstudio.com

#6 Val

Val

    Advanced Member

  • Members
  • PipPipPip
  • 53 posts
  • LocationNamibia and Denver

Posted 24 May 2013 - 08:57 AM

I have a recipe that is for firing at cone 04, stroke n' coats will lose none of their color at ^04. This recipe can be brushed to dipped, try to keep the application thin though.




Linda Arbuckle Majolica:

frit 3124 65.8

F-4 feldspar 17.2

EPK 10.8

neph sy 6.2

100.0

+ tin 4

+ zircopax 9

+ bentonite 2




#7 Val

Val

    Advanced Member

  • Members
  • PipPipPip
  • 53 posts
  • LocationNamibia and Denver

Posted 24 May 2013 - 08:59 AM

thanks all. Don't think we have liquid starch but maybe I can mix some. Is it way too soft otherwise?

#8 Nelly

Nelly

    Advanced Member

  • Members
  • PipPipPip
  • 380 posts

Posted 24 May 2013 - 09:21 AM

thanks all. Don't think we have liquid starch but maybe I can mix some. Is it way too soft otherwise?


Dear Val,

I have just used this recipe decorating some pots on the weekend. I must say, all and all, I was very, very pleased with the results.

I bisqued some redware to cone 04 and actually did the glaze using the Arbuckle to 04.

Yes, it is soft if what has been meant is that when you attempt to paint on the form, it is dusty and can pull the glaze of?? Not sure if that is what is meant by "soft."

I used a little glycerin to make my colors run more readily. I used commercial majolica glazes on my work.

But all and all, the glaze was great.

It performed as expected.

My greatest learning from this glaze at this point is that it is "all in the dip." You don't want drips on your work so your work must be exact in how you dip your vessels into the glaze. With beads, you should be fine.

Sounds like a great project.

Nelly

#9 Corinda Genev

Corinda Genev

    Member

  • Members
  • PipPip
  • 13 posts
  • LocationVancouver

Posted 08 July 2013 - 02:00 AM

spray with a stay flo laundry starch to harden the glaze surface before painting overglazes.
Linda has detailed handouts online.

Marcia

 

Marcia, could you point me in the direction of Linda's handouts. Thanks



#10 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 6,361 posts
  • LocationRed Lodge, Montana

Posted 08 July 2013 - 07:35 AM

here is the link. You just have to google Arbuckle handouts

 

arbuckle.com/arbuckle_handouts.html

 

Marcia


Marcia Selsor, Professor Emerita,Montana State University-Billings
[http://www.marciaselsorstudio.com




0 user(s) are reading this topic

0 members, 0 guests, 0 anonymous users